A reservoir bottom film with both plastic deformation and strength performance and its preparation process

By compounding high-density polyethylene resin with ethylene-vinyl acetate copolymer, and adding carbon black and titanium alloy plasma layers, the durability problem of the library bottom membrane under high water flow and drop impact is solved, and its mechanics and Anti-seepage performance ensures stable performance in various environments.

CN118496543BActive Publication Date: 2024-10-15SHANDONG JIANTONG PLASTIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962949.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-15
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing reservoir bottom membrane is prone to penetration failure and stress concentration, which leads to the performance degradation or failure of the anti-seepage system. It especially shows poor durability under conditions of high water flow and drop impact.

Method used

High-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer are used to compound, and by adding carbon black and titanium alloy plasma layers, the mechanical properties and anti-corrosion properties of the library bottom film are improved, and through modification treatment Improve the strength and aging resistance of materials.

Benefits of technology

The prepared reservoir bottom membrane has significantly improved mechanical properties, including high tensile strength, elongation at break and tear resistance. It can maintain good anti-seepage and anti-corrosion properties in various environments and is suitable for high water flow. and drop impact conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a reservoir bottom membrane that takes into account both plastic deformation and strength performance and a preparation process thereof, and relates to the field of geomembrane technology. The preparation process comprises the following steps: by mass percentage, 60%-70% of a raw material high-density polyethylene resin, 10%-30% of an ethylene-vinyl acetate copolymer, 10%-20% of a thermoplastic elastomer, 2%-5% of carbon black and 5%-10% of a stabilizer are melt-mixed and molded at 160°C-250°C to obtain a reservoir bottom membrane that takes into account both plastic deformation and strength performance. The reservoir bottom membrane prepared by the present invention has good mechanical properties and anti-seepage properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of geomembranes, and in particular to a reservoir bottom membrane having both plastic deformation and strength properties and a preparation process thereof. Background Art

[0002] As a special structure, water conservancy projects not only waste water resources, but also affect the stability of the dam. As a new type of artificial synthetic polymer material, geomembrane has good toughness, deformation resistance and ductility, which can help the dam withstand certain compressive stress and improve the stability of the dam.

[0003] Geomembrane is a waterproof barrier material based on high molecular polymer. It is mainly divided into low-density polyethylene (LDPE) geomembrane, high-density polyethylene (HDPE) geomembrane and EVA geomembrane. Geomembrane with a thickness greater than or equal to 0.8mm can also be called "waterproof board". Summary of the invention

[0004] The inventors have found that the existing reservoir bottom membrane is prone to penetration damage, and there is stress concentration at the connection of the reservoir bottom membrane, which is also prone to seam damage. This leads to a decline in the performance of the entire anti-seepage system or even failure. After many studies, the inventors have adopted high-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer, added carbon black, stabilizer and other additives, and compounded a series of raw materials to provide a reservoir bottom membrane that can ensure anti-seepage performance while taking into account plastic deformation, tear resistance and strength performance. The study found that the mechanical properties of a single LDPE reservoir bottom membrane are relatively poor. When the water flow height of the dam exceeds 100m, the reservoir bottom membrane has poor resistance to drop impact. The present application compounds high-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer. By adding an appropriate amount of ethylene-vinyl acetate copolymer, it can not only promote the good dispersion of the cross-linked thermoplastic elastomer in the resin phase, but also promote the mutual penetration between macromolecules, play a role in strengthening the interface between the two phases, and significantly enhance the effect of the two-phase interface, so that the reservoir bottom membrane finally prepared has good mechanical properties.

[0005] On the one hand, the present invention provides a preparation process for a reservoir bottom film that takes both plastic deformation and strength performance into consideration, the preparation process comprising the following steps: by mass percentage, 60%-70% of a raw material high-density polyethylene resin, 10%-30% of an ethylene-vinyl acetate copolymer, 10%-20% of a thermoplastic elastomer, 2%-5% of carbon black and 5%-10% of a stabilizer are melt-mixed and molded at 160° C.-250° C. to obtain a reservoir bottom film that takes both plastic deformation and strength performance into consideration.

[0006] Optionally, the mass ratio of the high-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer is (6-7): (1-2):1.

[0007] Optionally, the reservoir bottom membrane comprises a resin layer and a titanium alloy plasma layer deposited on the inner and outer surfaces of the resin layer, and the resin layer is prepared using the above raw materials;

[0008] The method for preparing the titanium alloy plasma layer comprises the following steps: (1) placing the resin layer in a vacuum chamber, introducing helium gas, and raising the pressure of the vacuum chamber to 8×10 -2 -1×10 -1 Pa, ionizing the helium gas under the action of a magnetic field and microwaves, and using the generated helium plasma to clean the resin layer;

[0009] (2) Then, 2%-8% titanium nanoalloy is introduced into the vacuum chamber to generate titanium alloy plasma under the activation of helium plasma; (3) The resin layer is adjusted to a positive bias voltage, and the titanium alloy plasma is deposited on the inner and outer surfaces of the resin layer to generate a titanium alloy plasma layer.

[0010] Optionally, the high-density polyethylene resin has a density greater than 1.5 g / cm 3 , the melt flow mass rate at 190°C and 2.16kg is less than 0.61g / 10min.

[0011] Optionally, the high-density polyethylene resin is subjected to a modification treatment, wherein the modification treatment comprises the following steps:

[0012] The dried high-density polyethylene resin, silicon carbide, magnesium sulfate and a silane coupling agent are blended, extruded and granulated to obtain a modified high-density polyethylene resin.

[0013] Wherein, the mass ratio of high-density polyethylene resin, silicon carbide, magnesium sulfate and silane coupling agent is (5-8):(1-3):(1-3):1.

[0014] Optionally, the thermoplastic elastomer is one or more of SBS, SIS, and SEBS.

[0015] Optionally, carbon black is 2%-5%, and the average particle size of the carbon black is less than 30nm.

[0016] Optionally, the carbon black is subjected to a modification treatment, and the modification treatment process comprises the following steps:

[0017] The sodium carbonate solution is added dropwise to the aqueous dispersion of carbon black, and the modified carbon black with a pH value of 8-10 is obtained through dehydration and drying.

[0018] Optionally, the stabilizer is one or more of 2,6-di-tert-butyl-4-methylphenol, antioxidant 1010, antioxidant 1076, and diisooctylphenyl phosphite.

[0019] On the other hand, the present invention provides a reservoir bottom film that takes both plastic deformation and strength properties into consideration, and the reservoir bottom film is prepared by the above-mentioned preparation method.

[0020] Compared with the prior art, the present invention achieves at least one of the following beneficial effects:

[0021] (1) The reservoir bottom film prepared by the present invention is prepared by compounding high-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer. By adding an appropriate amount of ethylene-vinyl acetate copolymer, it can not only promote the good dispersion of the cross-linked thermoplastic elastomer in the resin phase, but also promote the mutual penetration between macromolecules, play a role in strengthening the interface between the two phases, and significantly enhance the effect of the two-phase interface, so that the reservoir bottom film finally prepared has good mechanical properties.

[0022] (2) The reservoir bottom membrane prepared by the present invention is added with metallic titanium. The introduction of metallic titanium makes the reservoir bottom membrane have stronger anti-corrosion performance, so that the reservoir bottom membrane can be applied to various environments.

[0023] (3) The present invention improves the mechanical properties and aging resistance of the high-density polyethylene resin by modifying the high-density polyethylene resin and adding silicon carbide and magnesium sulfate to the high-density polyethylene resin, thereby further improving the strength performance of the reservoir bottom membrane.

[0024] (4) The present invention modifies carbon black, which is beneficial to the contact and infiltration of the resin and the carbon black, improves the bonding between the resin and the carbon black interface, enhances the mechanical properties of the carbon black filled resin, and further improves the mechanical properties of the reservoir bottom membrane. DETAILED DESCRIPTION

[0025] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below by way of examples.

[0026] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and therefore, the scope of protection of the present invention is not limited by the specific embodiments disclosed below. In the description of this specification, the description of reference terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily have to be directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0027] In an exemplary embodiment of the present invention, a preparation process for a reservoir bottom film having both plastic deformation and strength properties comprises the following steps: by mass percentage, 60%-70% of a raw material high-density polyethylene resin, 10%-30% of an ethylene-vinyl acetate copolymer, 10%-20% of a thermoplastic elastomer, 2%-5% of carbon black and 5%-10% of a stabilizer are melt-mixed and molded at 160°C-250°C to obtain a reservoir bottom film having both plastic deformation and strength properties.

[0028] Optionally, the preparation process comprises the following steps:

[0029] (1) Add the raw materials to the high-speed blender in proportion, stir to obtain the premix, select the co-rotating twin-screw extruder to blend and extrude the premix, heat the equipment during the twin-screw extruder processing, each heating zone is a partition, and different processing temperatures are set for each partition according to different processing technologies. At the same time, the barrel screw elements corresponding to each partition are also different; during processing, it can be divided into 4 to 6 zones, each zone includes 2 to 4 sub-zones, the processing temperature in the same sub-zone is uniform and unchanged, and the processing temperature of each zone increases in sequence. The material is evenly dispersed and the performance of each material is fully utilized. For example, the processing temperatures of zones 1 to 12 of the above-mentioned twin-screw extruder can be: zone 1 160°C, zone 2 160°C, zone 3 160°C, zone 4 160°C, zone 5 170°C, zone 6 170°C, zone 7 180°C, zone 8 180°C, zone 9 185°C, zone 10 185°C, zone 11 200°C, zone 12 200°C.

[0030] (2) The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine, and the screw temperatures of zones 1 to 5 of the blow molding machine are 180° C., 185° C., 190° C., 200° C., and 250° C., respectively, and the bottom film is obtained by extrusion molding.

[0031] Optionally, the mass ratio of the high-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer is (6-7): (1-2):1.

[0032] Optionally, the high-density polyethylene resin has a density greater than 1.5 g / cm 3 , the melt flow mass rate at 190°C and 2.16kg is less than 0.61.0g / 10min.

[0033] Optionally, the high-density polyethylene resin is subjected to a modification treatment, wherein the modification treatment comprises the following steps:

[0034] The dried high-density polyethylene resin, silicon carbide, magnesium sulfate and a silane coupling agent are blended, extruded and granulated to obtain a modified high-density polyethylene resin.

[0035] The mass ratio of high-density polyethylene resin, silicon carbide, magnesium sulfate and silane coupling agent is (5-8): (1-3): (1-3): 1. In the present invention, silicon carbide and magnesium sulfate are added to high-density polyethylene resin to improve the mechanical properties and anti-aging properties of high-density polyethylene resin, and further improve the strength performance of the bottom film. Optionally, the silane coupling agent can be one of methyltrichlorosilane, aminosilane, vinylsilane, epoxysilane and allyltrimethoxysilane.

[0036] Optionally, the thermoplastic elastomer is one or more of styrene-butadiene-styrene block copolymer (SBS for short), styrene-isoprene-styrene copolymer (SIS for short), and hydrogenated styrene-butadiene block copolymer (SEBS for short).

[0037] Optionally, carbon black is 2%-5%, and the average particle size of carbon black is less than 30nm. Preferably, the average particle size of carbon black is less than 20nm. A large amount of carbon black will reduce the mechanical properties of the bottom film, and carbon black within this range can ensure the mechanical properties of the bottom film. Using carbon black with a smaller particle size can effectively block ultraviolet rays and prevent ultraviolet degradation of the bottom film.

[0038] Optionally, the carbon black is subjected to a modification treatment, and the modification treatment process comprises the following steps:

[0039] Sodium carbonate solution is added dropwise to the aqueous dispersion of carbon black, and the modified carbon black with a pH of 8-10 is obtained after dehydration and drying. The modified carbon black has a looser structure and is easier to break and disperse during the compounding and kneading process with the raw materials, which is beneficial to the contact and infiltration of the resin and the carbon black, improves the bonding between the resin and the carbon black interface, enhances the mechanical properties of the carbon black filled resin, and further improves the mechanical properties of the bottom membrane.

[0040] Optionally, the stabilizer is one or more of 2,6-di-tert-butyl-4-methylphenol, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol (abbreviated as antioxidant 1076), and diisooctyl phenyl phosphite.

[0041] In another exemplary embodiment of the present invention, based on the above embodiment, the reservoir bottom film includes a resin layer and a titanium alloy plasma layer deposited on the inner and outer surfaces of the resin layer, and the resin layer can be the reservoir bottom film prepared as described above.

[0042] The method for preparing the titanium alloy plasma layer comprises the following steps: placing the resin layer in a vacuum chamber, introducing helium gas, and raising the pressure of the vacuum chamber to 8×10 -2 -1×10 -1 Pa, ionizing the helium gas under the action of a magnetic field and microwaves, and using the generated helium plasma to clean the resin layer;

[0043] Then, 2%-8% titanium nano-alloy is introduced into the vacuum chamber to generate titanium alloy plasma under the activation of helium plasma; the resin layer is adjusted to a positive bias voltage, and the titanium alloy plasma is deposited on the inner and outer surfaces of the resin layer to generate a titanium alloy plasma layer.

[0044] Specifically, the present invention first sends the prepared resin layer into a vacuum chamber, introduces helium gas and reaches stability, then turns on the magnetic coil current to generate a predetermined magnetic field, and turns on the microwave to couple it with the magnetic field to generate helium plasma; before coating, the resin layer is surface cleaned with helium plasma, and after cleaning, titanium nano-alloy is introduced, and the titanium nano-alloy is ionized under the action of helium plasma to form titanium alloy plasma, and then the power is turned on to bombard the surface of the resin layer to form electron irradiation, and the titanium alloy plasma is deposited on the surface of the resin layer, and a titanium alloy plasma layer is generated on the inner and outer surfaces of the resin layer under extremely low pressure to obtain a bottom film. The introduction of metallic titanium makes the bottom film have stronger anti-corrosion properties, so that the bottom film can be applied to various environments. Furthermore, the titanium nano-alloy forms a chemical bond with the resin layer during the plasma deposition process, which improves the bonding effect between the titanium alloy plasma layer and the resin system layer used in the ultra-low temperature liquid hydrogen environment, and ensures the interface compatibility.

[0045] Example 1

[0046] The preparation process of the bottom film of the reservoir taking into account both plastic deformation and strength performance includes the following steps:

[0047] (1) By mass percentage, the raw material high-density polyethylene resin is 60%, and the density of the high-density polyethylene resin is greater than 1.5g / cm 3, the melt flow mass rate at 190°C and 2.16kg is less than 0.61g / 10min, ethylene-vinyl acetate copolymer 10%, thermoplastic elastomer SBS 10%, carbon black 2%, carbon black average particle size 25nm, and antioxidant 1010 5% are added to a high-speed blender and stirred to obtain a premix, and a co-rotating twin-screw extruder is selected to blend and extrude the premix, and the processing temperatures of zones 1 to 12 of the twin-screw extruder can be respectively: zone 1 160°C, zone 2 160°C, zone 3 160°C, zone 4 160°C, zone 5 170°C, zone 6 170°C, zone 7 180°C, zone 8 180°C, zone 9 185°C, zone 10 185°C, zone 11 200°C, zone 12 200°C.

[0048] (2) The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine, and the screw temperatures of zones 1 to 5 of the blow molding machine are 180° C., 185° C., 190° C., 200° C., and 250° C., respectively, and the bottom film is obtained by blow molding.

[0049] Example 2

[0050] The preparation process of the bottom film of the reservoir taking into account both plastic deformation and strength performance includes the following steps:

[0051] (1) A high-density polyethylene resin is subjected to a modification treatment, wherein the modification treatment comprises the following steps: dry high-density polyethylene resin, silicon carbide, magnesium sulfate and silane coupling agent allyl trimethoxysilane are blended and extruded at a mass ratio of 5:1:1:1 at a temperature of 160-200° C., and granulated to obtain a modified high-density polyethylene resin.

[0052] The carbon black is modified, and the modification process includes the following steps: adding sodium carbonate solution dropwise into the water dispersion of the carbon black, and obtaining modified carbon black with a pH of 8 through dehydration and drying.

[0053] (2) By mass percentage, the raw material is modified into a high-density polyethylene resin of 65%, wherein the density of the modified high-density polyethylene resin is greater than 1.5 g / cm 3 , the melt flow mass rate at 190°C and 2.16kg is less than 0.61g / 10min, ethylene-vinyl acetate copolymer 20%, thermoplastic elastomer SIS 15%, modified carbon black 3%, modified carbon black average particle size 15nm, and 2,6-di-tert-butyl-4-methylphenol 7% are added to a high-speed blender and stirred to obtain a premix, and a co-rotating twin-screw extruder is selected to blend and extrude the premix, and the processing temperatures of zones 1 to 12 of the twin-screw extruder can be respectively: zone 1 160°C, zone 2 160°C, zone 3 160°C, zone 4 160°C, zone 5 170°C, zone 6 170°C, zone 7 180°C, zone 8 180°C, zone 9 185°C, zone 10 185°C, zone 11 200°C, zone 12 200°C.

[0054] (3) The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine, and the screw temperatures of zones 1 to 5 of the blow molding machine are 180° C., 185° C., 190° C., 200° C., and 250° C., respectively, and the bottom film is obtained by blow molding.

[0055] Example 3

[0056] The preparation process of the bottom film of the reservoir taking into account both plastic deformation and strength performance includes the following steps:

[0057] (1) A high-density polyethylene resin is subjected to a modification treatment, wherein the modification treatment comprises the following steps: dry high-density polyethylene resin, silicon carbide, magnesium sulfate and silane coupling agent vinyl silane are blended and extruded at a mass ratio of 6:1:2:1 at a temperature of 160-200° C., and granulated to obtain a modified high-density polyethylene resin.

[0058] The carbon black is modified, and the modification process includes the following steps: adding sodium carbonate solution dropwise into the water dispersion of the carbon black, and obtaining modified carbon black with a pH of 9 through dehydration and drying.

[0059] (2) By mass percentage, 70% of the raw material is modified high-density polyethylene resin, wherein the density of the modified high-density polyethylene resin is greater than 1.5 g / cm 3 , the melt flow mass rate at 190°C and 2.16kg is less than 0.61g / 10min, ethylene-vinyl acetate copolymer 20%, thermoplastic elastomer SIS 10%, modified carbon black 4%, modified carbon black average particle size 17nm, and monoisooctyl phenyl phosphite 7% are added to a high-speed blender and stirred to obtain a premix, and a co-rotating twin-screw extruder is selected to blend and extrude the premix, and the processing temperatures of zones 1 to 8 of the twin-screw extruder can be respectively: zone 1 170°C, zone 2 170°C, zone 3 180°C, zone 4 180°C, zone 5 185°C, zone 6 185°C, zone 7 200°C, zone 8 200°C.

[0060] (3) The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine, and the screw temperatures of zones 1 to 4 of the blow molding machine are 180° C., 185° C., 190° C., and 200° C., respectively, and the bottom film is obtained by blow molding.

[0061] Example 4

[0062] The preparation process of the bottom film of the reservoir taking into account both plastic deformation and strength performance includes the following steps:

[0063] (1) A high-density polyethylene resin is subjected to a modification treatment, wherein the modification treatment comprises the following steps: dry high-density polyethylene resin, silicon carbide, magnesium sulfate and silane coupling agent aminosilane are blended and extruded at a mass ratio of 8:3:2:1 at a temperature of 160-200° C., and granulated to obtain a modified high-density polyethylene resin.

[0064] The carbon black is modified, and the modification process includes the following steps: adding sodium carbonate solution dropwise into the water dispersion of the carbon black, and obtaining modified carbon black with a pH of 10 through dehydration and drying.

[0065] (2) By mass percentage, 70% of the raw material is modified high-density polyethylene resin, wherein the density of the modified high-density polyethylene resin is greater than 1.5 g / cm 3 , the melt flow mass rate at 190°C and 2.16kg is less than 0.61g / 10min, ethylene-vinyl acetate copolymer 30%, thermoplastic elastomer SEBS 15%, modified carbon black 4%, modified carbon black average particle size 15nm, and antioxidant 1076 10% are added to a high-speed blender and stirred to obtain a premix, and a co-rotating twin-screw extruder is selected to blend and extrude the premix, and the processing temperatures of zones 1 to 8 of the twin-screw extruder can be respectively: zone 1 170°C, zone 2 170°C, zone 3 180°C, zone 4 180°C, zone 5 185°C, zone 6 185°C, zone 7 200°C, zone 8 200°C.

[0066] (3) The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine, and the screw temperatures of zones 1 to 4 of the blow molding machine are 180° C., 185° C., 190° C., and 200° C., respectively, and the bottom film is obtained by extrusion molding.

[0067] Example 5

[0068] The preparation process of the bottom film of the reservoir taking into account both plastic deformation and strength performance includes the following steps:

[0069] Based on Example 2, the main difference is that the reservoir bottom film includes a resin layer and a titanium alloy plasma layer deposited on the inner and outer surfaces of the resin layer. The reservoir bottom film prepared in Example 2 is used as the resin layer.

[0070] The resin layer was placed in a vacuum chamber and 5 sccm of helium was introduced to raise the pressure of the vacuum chamber to 9×10 -2 Pa, under the action of a magnetic field and a 600W microwave, the helium gas is ionized to generate helium plasma, a negative bias voltage of 40V is set, and the generated helium plasma is used to clean the resin layer.

[0071] Then, 2% titanium nano-alloy is introduced into the vacuum chamber to generate titanium alloy plasma under the activation of helium plasma.

[0072] The resin layer is then adjusted to a positive bias voltage of 50 V. The positive bias voltage is used to achieve electron irradiation, and titanium alloy plasma is deposited on the inner and outer surfaces of the resin layer to generate a titanium alloy plasma layer.

[0073] Example 6

[0074] The preparation process of the bottom film of the reservoir taking into account both plastic deformation and strength performance includes the following steps:

[0075] Based on Example 2, the main difference is that the reservoir bottom film includes a resin layer and a titanium alloy plasma layer deposited on the inner and outer surfaces of the resin layer. The reservoir bottom film prepared in Example 2 is used as the resin layer.

[0076] The resin layer was placed in a vacuum chamber and 7 sccm of helium was introduced to raise the pressure of the vacuum chamber to 11×10 -2 Pa, under the action of a magnetic field and a 600W microwave, the helium gas is ionized to generate helium plasma, a negative bias voltage of 70V is set, and the generated helium plasma is used to clean the resin layer.

[0077] Then, 5% titanium nano-alloy is introduced into the vacuum chamber to generate titanium alloy plasma under the activation of helium plasma.

[0078] The resin layer is then adjusted to a positive bias voltage of 70 V. The positive bias voltage is used to achieve electron irradiation, and titanium alloy plasma is deposited on the inner and outer surfaces of the resin layer to generate a titanium alloy plasma layer.

[0079] Example 7

[0080] The main difference from Example 2 is that the carbon black is not modified.

[0081] Comparative Example 1

[0082] Based on Example 1, the main difference is that no thermoplastic elastomer is added in the preparation process of the bottom film.

[0083] Comparative Example 2

[0084] Based on Example 1, the main difference is that no ethylene-vinyl acetate copolymer is added in the reservoir bottom film preparation process.

[0085] The bottom membranes prepared in Examples 1-7 and Comparative Examples 1-2 were subjected to performance tests. The thickness of the bottom membranes was 2 mm, and the tensile strength and elongation at break were tested in accordance with GB / T17632 and GB / T1040.2-2006; the angular tear strength was tested in accordance with GB / T17632 and QB / T1130, with a test speed of 200 mm / min; the puncture resistance was tested in accordance with GB / T17632 and Appendix D of GB / T17643-2011, with a test speed of 300 mm / min; the anti-seepage performance was tested in accordance with GB / T17632 and GB / T328.10, and the test results are shown in Table 1.

[0086] Table 1 Performance test table

[0087]

[0088] As shown in Table 1, it can be seen that the mechanical properties of the reservoir bottom membrane prepared by the present invention are significantly improved, the elongation at break is not less than 800%, the tensile strength is not less than 50 kN / m, the right-angle tear load is not less than 300 N, the puncture resistance is not less than 600 N, there is no leakage at 0.3 MPa ≥ 24 h, and it has good anti-seepage performance.

[0089] At room temperature, the reservoir bottom membranes prepared in Examples 1-7 were placed in a corrosive solution of seawater, 50% benzene, 50% sulfuric acid and 20% sodium hydroxide. Although the mechanical properties of the reservoir bottom membranes decreased, the mechanical property retention rates of the reservoir bottom membranes were all above 95%, and the mechanical property retention rates of the reservoir bottom membranes in Examples 5-6 were all above 98%.

[0090] Compared with Example 1, in Comparative Example 2, since ethylene-vinyl acetate copolymer is not added, the thermoplastic elastomer cannot be completely cross-linked and dispersed in the resin phase, so that the mechanical properties of the reservoir bottom film finally prepared are reduced.

[0091] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A preparation process for a reservoir bottom film that takes into account both plastic deformation and strength performance, characterized in that: The preparation process comprises the following steps: by mass percentage, 60%-70% of a raw material high-density polyethylene resin, 10%-30% of an ethylene-vinyl acetate copolymer, 10%-20% of a thermoplastic elastomer, 2%-5% of carbon black and 5%-10% of a stabilizer are melt-mixed and molded at 160° C.-250° C. to obtain a bottom film having both plastic deformation and strength properties; The reservoir bottom film comprises a resin layer and a titanium alloy plasma layer deposited on the inner and outer surfaces of the resin layer; The method for preparing the titanium alloy plasma layer comprises the following steps: placing the resin layer in a vacuum chamber, introducing helium gas, and raising the pressure of the vacuum chamber to 8×10 -2 -1×10 -1 Pa, ionizing the helium gas under the action of a magnetic field and microwaves, and using the generated helium plasma to clean the resin layer; Then, 2%-8% of titanium nano alloy is introduced into the vacuum chamber to generate titanium alloy plasma under the activation of helium plasma; the resin layer is adjusted to a positive bias voltage, and the titanium alloy plasma is deposited on the inner and outer surfaces of the resin layer to generate a titanium alloy plasma layer; The high-density polyethylene resin is subjected to a modification treatment, wherein the modification treatment comprises the following steps: The dried high-density polyethylene resin, silicon carbide, magnesium sulfate and a silane coupling agent are blended, extruded and granulated to obtain a modified high-density polyethylene resin; Wherein, the mass ratio of high-density polyethylene resin, silicon carbide, magnesium sulfate and silane coupling agent is (5-8):(1-3):(1-3):

1.

2. The preparation process according to claim 1, characterized in that: The mass ratio of the high-density polyethylene resin, ethylene-vinyl acetate copolymer and thermoplastic elastomer is (6-7): (1-2):

1.

3. The preparation process according to claim 1, characterized in that: The high-density polyethylene resin has a density greater than 1.5 g / cm 3 , the melt flow mass rate at 190°C and 2.16kg is less than 0.61g / 10min.

4. The preparation process according to claim 1, characterized in that: The thermoplastic elastomer is one or more of SBS, SIS and SEBS.

5. The preparation process according to claim 1, characterized in that: Carbon black 2%-5%, the average particle size of carbon black is less than 30nm.

6. The preparation process according to claim 5, characterized in that: The carbon black is modified, and the modification process includes the following steps: The sodium carbonate solution is added dropwise to the aqueous dispersion of carbon black, and the modified carbon black with a pH value of 8-10 is obtained through dehydration and drying.

7. The preparation process according to claim 1, characterized in that: The stabilizer is one or more of 2,6-di-tert-butyl-4-methylphenol, antioxidant 1010, antioxidant 1076, and diisooctylphenyl phosphite.

8. A bottom membrane with both plastic deformation and strength properties, characterized in that: The reservoir bottom film is prepared by any one of the preparation methods of claims 1-7.