Light emitting diode epitaxial wafer and preparation method thereof, LED

By depositing Si3N4, BN and Mg3N2/BGaN superlattice layers on the multi-quantum well layer of the GaN layer, filling the V-shaped pit, the dislocation problem of gallium nitride film in heteroepitaxy growth is solved, and GaN-based photoelectricity is improved The device's photoelectric performance and reliability improve the luminous efficiency and stability of the light emitting diode.

CN118522835BActive Publication Date: 2024-11-12JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985764.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

During the heteroepitaxial growth of the gallium nitride film, V-shaped pit formation caused by lattice mismatch and thermal mismatch, resulting in low photoelectric performance and poor reliability of GaN-based photoelectric devices, and it is difficult for the prior art to effectively improve the luminescence of light-emitting diodes. Efficiency and stability.

Method used

The Si3N4 layer, BN layer, and Mg3N2/BGaN superlattice layer are deposited on the multi-quantum well layer of the GaN layer to fill the V-shaped pit, reduce dislocations and defects, and improve crystal quality and luminous efficiency.

Benefits of technology

By filling the V-shaped pit and reducing the dislocation density, the non-radiative composite center is reduced, the luminous efficiency and aging performance of the light emitting diode are improved, the leakage is reduced, and the photoelectric efficiency and electrical performance of the LED are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118522835B_ABST
    Figure CN118522835B_ABST
Patent Text Reader

Abstract

The present invention discloses a light emitting diode epitaxial wafer and a preparation method thereof, and an LED. The light emitting diode epitaxial wafer comprises a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged; the multi-quantum well layer has a V-shaped pit, a composite layer is deposited on the V-shaped pit, and the composite layer comprises Si deposited on the V-shaped pit in sequence. 3 N 4 layer, BN layer and Mg 3 N 2 / BGaN superlattice layer. The light-emitting diode epitaxial wafer provided by the present invention can avoid the formation of non-radiative recombination centers by dislocations in V-shaped pits, reduce leakage current of the light-emitting diode, and improve the light-emitting efficiency of the light-emitting diode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of optoelectronic technology, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and an LED. Background Art

[0002] Gallium nitride is a typical representative of the third generation of wide bandgap semiconductor materials. High-quality gallium nitride films are a key factor in the preparation of high-performance optoelectronic devices. At present, inexpensive sapphire has been widely used as a heteroepitaxial substrate for the epitaxial growth of gallium nitride films. Due to the large lattice mismatch and thermal mismatch between sapphire and gallium nitride, heteroepitaxially grown gallium nitride films have large residual stress and high dislocation density. These dislocations form a large number of V-shaped pits in the GaN epitaxial layer, and the dislocations in the V-shaped pits make GaN-based optoelectronic devices have disadvantages such as low optoelectronic performance and poor reliability. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a light emitting diode epitaxial wafer, which can avoid the formation of non-radiative recombination centers due to dislocations in V-pits, reduce leakage current of the light emitting diode, and improve the luminous efficiency of the light emitting diode.

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a light emitting diode epitaxial wafer, which has a simple process and can stably prepare a light emitting diode epitaxial wafer with good luminous efficiency.

[0005] In order to solve the above technical problems, the present invention provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged;

[0006] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0007] In one embodiment, the thickness of the Si3N4 layer is 1 nm to 10 nm.

[0008] In one embodiment, the thickness of the BN layer is 1 nm to 10 nm.

[0009] In one embodiment, the Mg3N2 / BGaN superlattice layer includes Mg3N2 layers and BGaN layers that are alternately stacked, and the number of the alternating stacking periods is 1 to 20.

[0010] In one embodiment, the thickness of the Mg3N2 layer is 0.5nm~5nm.

[0011] In one embodiment, the BGaN layer has a thickness of 1 nm to 10 nm.

[0012] In one embodiment, the B component of the BGaN layer is 0.01-0.1.

[0013] To solve the above problems, the present invention also provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:

[0014] S1. providing a substrate;

[0015] S2, depositing a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence;

[0016] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0017] In one embodiment, the steps include:

[0018] providing a substrate;

[0019] depositing a buffer layer on the substrate;

[0020] Depositing a non-doped GaN layer on the buffer layer;

[0021] Depositing an N-type GaN layer on the undoped GaN layer;

[0022] Depositing a multi-quantum well layer on the N-type GaN layer, wherein the multi-quantum well layer has V-shaped pits;

[0023] Depositing a composite layer on the V-shaped pit, wherein the composite layer fills the V-shaped pit;

[0024] depositing an electron blocking layer on the multi-quantum well layer and the composite layer;

[0025] A P-type GaN layer is deposited on the electron blocking layer.

[0026] Correspondingly, the present invention further provides an LED, which includes the above-mentioned light emitting diode epitaxial wafer.

[0027] The implementation of the present invention has the following beneficial effects:

[0028] The light-emitting diode epitaxial wafer provided by the present invention has a multi-quantum well layer with a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer deposited in sequence on the V-shaped pit.

[0029] The GaN layer is deposited on a heterogeneous substrate, and a V-shaped pit is formed due to dislocations generated by lattice mismatch. Therefore, the multi-quantum well layer has a V-shaped pit. Depositing a Si3N4 layer on the V-shaped pit can reduce the extension of the screw dislocation at the bottom of the V-shaped pit to the P-type GaN layer, improve the crystal quality of the P-type GaN layer, reduce the leakage of the light-emitting diode, and improve the aging performance. Then the deposition of the BN layer can block the dislocations that partially penetrate the Si3N4 layer for a second time, further reduce the dislocation density of the P-type GaN layer, reduce the defect-trapped holes, and reduce non-radiative recombination. Finally, the B of the BGaN layer of the Mg3N2 / BGaN superlattice layer reduces Mg passivation, increases the activated Mg concentration and hole concentration, increases the injection efficiency of the V-shaped pit sidewall, and improves the luminous efficiency of the light-emitting diode. In addition, the BGaN layer gradually fills the V-shaped pit to obtain a relatively smooth epitaxial layer plane, reducing the leakage of the light-emitting diode. The above avoids the formation of non-radiative recombination centers by dislocations in the V-shaped pit, reduces the leakage of the light-emitting diode, and improves the luminous efficiency of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram of the structure of a light emitting diode epitaxial wafer provided by the present invention;

[0031] Figure 2 A process flow chart of the method for preparing a light emitting diode epitaxial wafer provided by the present invention;

[0032] Figure 3 Another process flow chart of the method for preparing the light emitting diode epitaxial wafer provided by the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0034] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0035] In the present invention, “preferred” is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the protection scope of the present invention.

[0036] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0037] In the present invention, when a numerical range is involved, unless otherwise specified, the two endpoints of the numerical range are included.

[0038] The GaN layer is deposited on a foreign substrate, and V-shaped pits are formed due to dislocations caused by lattice mismatch. The dislocations in the V-shaped pits make GaN-based optoelectronic devices have disadvantages such as low optoelectronic performance and poor reliability.

[0039] To solve the above problems, the present invention provides a light emitting diode epitaxial wafer, such as Figure 1 As shown, it includes a substrate 100, on which a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, a multi-quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 are sequentially arranged;

[0040] The multi-quantum well layer 500 has a V-shaped pit 510 , on which a composite layer 800 is deposited. The composite layer 800 includes a Si 3 N 4 layer 810 , a BN layer 820 , and a Mg 3 N 2 / BGaN superlattice layer 830 which are sequentially deposited on the V-shaped pit 510 .

[0041] The specific structure of the composite layer 800 is as follows:

[0042] In one embodiment, the thickness of the Si3N4 layer 810 is 1 nm to 10 nm; exemplary thicknesses of the Si3N4 layer 810 are 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, and 9 nm, but are not limited thereto. Depositing the Si3N4 layer on the V-shaped pit can reduce the extension of the screw dislocation at the bottom of the V-shaped pit to the P-type GaN layer, improve the crystal quality of the P-type GaN layer, reduce the leakage of the light-emitting diode, and improve the aging performance.

[0043] In one embodiment, the thickness of the BN layer 820 is 1 nm to 10 nm, and exemplary thicknesses of the BN layer 820 are 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, and 9 nm, but are not limited thereto. Depositing the BN layer can block dislocations that partially penetrate the Si3N4 layer, further reduce the dislocation density of the P-type GaN layer, reduce defect-trapped holes, and reduce non-radiative recombination.

[0044] In one embodiment, the Mg3N2 / BGaN superlattice layer 830 includes Mg3N2 layers and BGaN layers alternately stacked, and the number of alternating stacking periods is 1 to 20. Exemplary numbers of alternating stacking periods are 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, but are not limited thereto. In one embodiment, the thickness of the Mg3N2 layer is 0.5nm to 5nm; the exemplary thickness of the Mg3N2 layer is 1nm, 1.5nm, 2nm, 2.5nm, 3nm, 3.5nm, 4nm, but are not limited thereto. In one embodiment, the thickness of the BGaN layer is 1nm to 10nm, and the exemplary thickness of the BGaN layer is 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, but are not limited thereto. In one embodiment, the B component of the BGaN layer is 0.01~0.1. In one embodiment, the composite layer 800 fills the V-shaped pit 510. Specifically, the Mg3N2 / BGaN superlattice layer of the composite layer 800 fills the V-shaped pit 510. The B of the BGaN layer of the Mg3N2 / BGaN superlattice layer 830 reduces Mg passivation, increases the activated Mg concentration and the hole concentration, increases the injection efficiency of the V-shaped pit sidewall, and increases the luminous efficiency of the light-emitting diode. In addition, the BGaN layer gradually fills the V-shaped pit to obtain a smoother epitaxial layer plane, thereby reducing the leakage of the light-emitting diode. The above avoids the formation of non-radiative recombination centers in the V-shaped pit, reduces the leakage of the light-emitting diode, and improves the luminous efficiency of the light-emitting diode.

[0045] In summary, the present invention can avoid the formation of non-radiative recombination centers due to dislocations in V-shaped pits by inserting a composite layer 800 with a specific structure, thereby reducing leakage current of the light-emitting diode and improving the light-emitting efficiency of the light-emitting diode.

[0046] Accordingly, the present invention provides a method for preparing a light emitting diode epitaxial wafer, such as Figure 2 As shown, the following steps are included:

[0047] S1, providing a substrate 100;

[0048] The substrate 100 may be selected from one of a sapphire substrate, a SiO2 sapphire composite substrate, a silicon substrate, a silicon carbide substrate, a gallium nitride substrate, and a zinc oxide substrate. Preferably, the substrate 100 is a sapphire substrate, which is a commonly used GaN-based LED substrate material. The sapphire substrate has a mature preparation process, a low price, is easy to clean and handle, and has good stability at high temperatures.

[0049] S2, sequentially depositing a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, a multi-quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 on the substrate 100;

[0050] The multi-quantum well layer 500 has a V-shaped pit 510 , on which a composite layer 800 is deposited. The composite layer 800 includes a Si 3 N 4 layer 810 , a BN layer 820 , and a Mg 3 N 2 / BGaN superlattice layer 830 which are sequentially deposited on the V-shaped pit 510 .

[0051] like Figure 3 As shown, the above preparation method specifically comprises the following steps:

[0052] S20, providing a substrate 100;

[0053] S21 , depositing the buffer layer 200 on the substrate 100 .

[0054] In one embodiment, the buffer layer 200 is an AlN buffer layer.

[0055] S22 , depositing the undoped GaN layer 300 on the buffer layer 200 .

[0056] In one embodiment, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, N source and Ga source are introduced, and a non-doped GaN layer with a thickness of 1 μm to 5 μm is grown.

[0057] S23 , depositing the N-type GaN layer 400 on the undoped GaN layer 300 .

[0058] In one embodiment, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Ga source, and a Si source are introduced to grow the N-type GaN layer.

[0059] S24 , depositing the multi-quantum well layer 500 on the N-type GaN layer 400 , wherein the multi-quantum well layer 500 has V-shaped pits 510 .

[0060] In one embodiment, the multi-quantum well layer includes a plurality of alternately stacked InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period number of 6 to 12, wherein the growth temperature of the InGaN quantum well layer is 790°C to 810°C, the thickness is 2nm to 5nm, and the growth pressure is 50torr to 300torr, and the growth temperature of the AlGaN quantum barrier layer is 800°C to 900°C, the thickness is 5nm to 15nm, and the growth pressure is 50torr to 300torr.

[0061] It should be noted that when GaN material is deposited on a foreign substrate, dislocations are generated due to lattice mismatch to form V-shaped pits. Therefore, the multi-quantum well layer has V-shaped pits, and the dislocations in the V-shaped pits make GaN-based optoelectronic devices have disadvantages such as low optoelectronic performance and poor reliability.

[0062] S25, depositing the composite layer 800 on the V-shaped pit 510, wherein the composite layer 800 fills the V-shaped pit 510;

[0063] In one embodiment, the Si3N4 layer 810 is prepared by:

[0064] The temperature of the reaction chamber is controlled at 800° C. to 900° C., the pressure is controlled at 50 torr to 500 torr, N source and Si source are introduced to grow the Si 3 N 4 layer.

[0065] In one embodiment, the BN layer 820 is prepared by:

[0066] The temperature of the reaction chamber is controlled at 800° C. to 900° C., the pressure is controlled at 50 torr to 500 torr, an N source and a B source are introduced, and the BN layer is grown.

[0067] In one embodiment, the Mg3N2 / BGaN superlattice layer 830 is prepared by:

[0068] The Mg3N2 / BGaN superlattice layer 830 includes Mg3N2 layers and BGaN layers alternately stacked, and the number of cycles of the alternate stacking is 1 to 20;

[0069] The Mg3N2 layer is prepared by the following method: the temperature of the reaction chamber is controlled at 800°C-900°C, the pressure is controlled at 50torr-500torr, N source and Mg source are introduced, and the Mg3N2 layer is grown.

[0070] The BGaN layer is prepared by the following method: the temperature of the reaction chamber is controlled at 800° C. to 900° C., the pressure is controlled at 50 torr to 500 torr, an N source, a Ga source and a B source are introduced to grow the BGaN layer.

[0071] S26, depositing the electron blocking layer 600 on the multi-quantum well layer 500 and the composite layer 800;

[0072] In one embodiment, the temperature of the reaction chamber is controlled at 900° C. to 1000° C., the pressure is controlled at 100 torr to 300 torr, N source, Al source, Ga source, and In source are introduced, and an AlInGaN electron blocking layer with a thickness of 10 nm to 40 nm is grown.

[0073] S27 , depositing the P-type GaN layer 700 on the electron blocking layer 600 .

[0074] In one embodiment, the temperature of the reaction chamber is controlled at 900° C. to 1050° C., the pressure is controlled at 100 torr to 600 torr, and N source, Mg source, Ga source, and In source are introduced to grow the P-type GaN layer.

[0075] Accordingly, the present invention further provides an LED, which comprises the above-mentioned light-emitting diode epitaxial wafer, wherein the photoelectric efficiency of the LED is effectively improved and other electrical properties are good.

[0076] The present invention is further described below with specific embodiments:

[0077] Example 1

[0078] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0079] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0080] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.05.

[0081] Example 2

[0082] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0083] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0084] Among them, the thickness of the Si3N4 layer is 3.5nm, the thickness of the BN layer is 1.5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.05.

[0085] Example 3

[0086] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0087] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0088] Among them, the thickness of the Si3N4 layer is 9.5nm, the thickness of the BN layer is 5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.05.

[0089] Example 4

[0090] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0091] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0092] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 1nm, the thickness of the BGaN layer is 3nm, and the B component of the BGaN layer is 0.05.

[0093] Example 5

[0094] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0095] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0096] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 4nm, the thickness of the BGaN layer is 8nm, and the B component of the BGaN layer is 0.05.

[0097] Example 6

[0098] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0099] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0100] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.07.

[0101] Example 7

[0102] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0103] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0104] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 10 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.02.

[0105] Example 8

[0106] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0107] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0108] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 15 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.05.

[0109] Example 9

[0110] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;

[0111] The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

[0112] Among them, the thickness of the Si3N4 layer is 6.5nm, the thickness of the BN layer is 3.5nm, and the Mg3N2 / BGaN superlattice layer includes 5 periods of alternating Mg3N2 layers and BGaN layers, among which the thickness of the Mg3N2 layer is 2.5nm, the thickness of the BGaN layer is 6nm, and the B component of the BGaN layer is 0.05.

[0113] Comparative Example 1

[0114] This comparative example provides a light-emitting diode epitaxial wafer, which is different from the rest of Example 1 in that: the composite layer includes a BN layer and a Mg3N2 / BGaN superlattice layer deposited sequentially on the V-shaped pit, and the rest is the same as Example 1.

[0115] Comparative Example 2

[0116] This comparative example provides a light-emitting diode epitaxial wafer, and the difference between the remaining embodiment 1 is that: the composite layer includes a Si3N4 layer and a Mg3N2 / BGaN superlattice layer deposited in sequence on the V-shaped pit, and the rest refers to embodiment 1.

[0117] Comparative Example 3

[0118] This comparative example provides a light-emitting diode epitaxial wafer, and the difference between the remaining embodiment 1 is that: the composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 layer deposited in sequence on the V-shaped pit, and the rest refers to embodiment 1.

[0119] Comparative Example 4

[0120] This comparative example provides a light-emitting diode epitaxial wafer, and the difference between the remaining embodiment 1 is that: the composite layer includes a Si3N4 layer, a BN layer and a BGaN layer deposited in sequence on the V-shaped pit, and the rest refers to embodiment 1.

[0121] The light-emitting diode epitaxial wafers prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were used to prepare 10 mil×24 mil chips using the same chip process conditions. 300 LED chips were respectively extracted and tested at a current of 120 mA. Compared with the LEDs prepared from the light-emitting diode epitaxial wafers without the composite layer, the luminous efficiency improvement rate of each embodiment and comparative example was calculated. The specific test results are shown in Table 1.

[0122] Table 1 Performance test results of LEDs obtained from Examples 1 to 9 and Comparative Examples 1 to 4

[0123]

[0124] From the above results, it can be seen that the light-emitting diode epitaxial wafer provided by the present invention has a multi-quantum well layer with a V-shaped pit, and a composite layer is deposited on the V-shaped pit, and the composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer deposited in sequence on the V-shaped pit.

[0125] The GaN layer is deposited on a heterogeneous substrate, and a V-shaped pit is formed due to dislocations generated by lattice mismatch. Therefore, the multi-quantum well layer has a V-shaped pit. Depositing a Si3N4 layer on the V-shaped pit can reduce the extension of the screw dislocation at the bottom of the V-shaped pit to the P-type GaN layer, improve the crystal quality of the P-type GaN layer, reduce the leakage of the light-emitting diode, and improve the aging performance. Then the deposition of the BN layer can block the dislocations that partially penetrate the Si3N4 layer for a second time, further reduce the dislocation density of the P-type GaN layer, reduce the defect-trapped holes, and reduce non-radiative recombination. Finally, the B of the BGaN layer of the Mg3N2 / BGaN superlattice layer reduces Mg passivation, increases the activated Mg concentration and hole concentration, increases the injection efficiency of the V-shaped pit sidewall, and improves the luminous efficiency of the light-emitting diode. In addition, the BGaN layer gradually fills the V-shaped pit to obtain a relatively smooth epitaxial layer plane, reducing the leakage of the light-emitting diode. The above avoids the formation of non-radiative recombination centers by dislocations in the V-shaped pit, reduces the leakage of the light-emitting diode, and improves the luminous efficiency of the light-emitting diode.

[0126] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged; The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer fills the V-shaped pit, and the composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the Si3N4 layer is 1nm~10nm.

3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the BN layer is 1 nm to 10 nm.

4. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The Mg3N2 / BGaN superlattice layer includes Mg3N2 layers and BGaN layers that are alternately stacked, and the number of cycles of the alternate stacking is 1 to 20.

5. The light emitting diode epitaxial wafer according to claim 4, characterized in that: The thickness of the Mg3N2 layer is 0.5nm~5nm.

6. The light emitting diode epitaxial wafer according to claim 4, characterized in that: The thickness of the BGaN layer is 1 nm to 10 nm.

7. The light emitting diode epitaxial wafer according to claim 4, characterized in that: The B component of the BGaN layer is 0.01-0.

1.

8. A method for preparing a light emitting diode epitaxial wafer according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. providing a substrate; S2, depositing a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence; The multi-quantum well layer has a V-shaped pit, and a composite layer is deposited on the V-shaped pit. The composite layer includes a Si3N4 layer, a BN layer and a Mg3N2 / BGaN superlattice layer sequentially deposited on the V-shaped pit.

9. The method for preparing a light emitting diode epitaxial wafer according to claim 8, characterized in that: The following steps are involved: providing a substrate; depositing a buffer layer on the substrate; Depositing a non-doped GaN layer on the buffer layer; Depositing an N-type GaN layer on the undoped GaN layer; Depositing a multi-quantum well layer on the N-type GaN layer, wherein the multi-quantum well layer has V-shaped pits; Depositing a composite layer on the V-shaped pit, wherein the composite layer fills the V-shaped pit; depositing an electron blocking layer on the multi-quantum well layer and the composite layer; A P-type GaN layer is deposited on the electron blocking layer.

10. An LED, characterized in that: The LED comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 7.