Surface spraying technology of NdFeB magnets for automotive sensors

By pretreatment and optimization of spraying parameters, combined with the crosslinking reaction between diluent and filling liquid, the problem of insufficient coating uniformity and binding force of NdFeB magnets is solved, and efficient and uniform coating preparation is achieved, reducing magnetic properties The impact of

CN118527328BActive Publication Date: 2024-11-19ARCFL TECH LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014149.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-19
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing neodymium iron boron magnet spraying process has problems such as poor coating uniformity, insufficient binding force, and great impact on magnetism. In addition, traditional air spraying processes require strict control of spraying parameters, affecting production efficiency.

Method used

Pretreatment steps include degreasing, oil removal, pickling and rust removal and hole sealing filling, air spraying using diluted epoxy resin coating, adjusting spray parameters such as spray gun angle, distance, speed and curing conditions, and combining with Ethyl in the diluent The dialdehyde is cross-linked with the polyvinyl alcohol in the filling solution to improve the density and corrosion resistance of the coating.

Benefits of technology

The uniformity, bonding force and corrosion resistance of the coating are improved, while reducing the impact on the magnetic properties of neodymium iron boron magnets and improving production efficiency. The coating thickness is 10-15μm, with excellent mechanical properties and corrosion resistance. sex.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of NdFeB magnet spraying, and specifically relates to a surface spraying process of NdFeB magnets for automotive sensors. The spraying process comprises the following steps: soaking the NdFeB magnet in a mixed aqueous solution of sodium carbonate and sodium hydroxide for degreasing and oil removal; soaking the NdFeB magnet after degreasing and oil removal in an acid solution for pickling and rust removal; soaking the NdFeB magnet after pickling and rust removal in a filling liquid containing polyvinyl alcohol, silane coupling agent, and nano-silicon dioxide for hole sealing and filling; placing the NdFeB magnet after hole sealing and filling on a spraying platform, and spraying on both sides with epoxy resin coating diluted with a diluent to obtain a coating with a thickness of 10-15 μm. The present invention pre-treats the NdFeB magnet and adjusts the spraying process parameters, so that the prepared coating has good uniformity, high bonding force, good corrosion resistance, and little influence on the magnetism of the NdFeB magnet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of NdFeB magnet spraying, and in particular relates to a surface spraying process for NdFeB magnetic steel of automobile sensors. Background Art

[0002] Neodymium iron boron (NdFeB) alloy is an excellent permanent magnetic material with high magnetic energy product, good magnetic properties and chemical stability. It is widely used in motors, generators, sensors and other fields. Surface spraying is a commonly used surface treatment process. Surface spraying of NdFeB materials can improve their corrosion resistance and wear resistance.

[0003] Spraying is a coating method that uses a spray gun or a disc atomizer to disperse the paint into uniform and fine droplets with the help of pressure or centrifugal force, and then applies it to the surface of the product. It includes air spraying, airless spraying, electrostatic spraying, etc. Among them, air spraying is the most commonly used spraying method. Compared with other spraying methods, air spraying has the following advantages: (1) Air spraying is suitable for long-term work, and there is no situation where the motor overheats and cannot work normally; (2) Air spraying only has a pressure source, there is no risk of electric shock, and the spraying equipment itself does not generate sparks; (3) The maintenance cost of air spraying equipment is much lower than that of electrostatic spraying; (4) There are no specific requirements for the conductivity of the paint and solvent, and the volatility of the solvent, while electrostatic spraying requires the use of special paint.

[0004] However, the traditional air spraying process is to spray the coating by moving the spray gun, which requires strict control of the spraying process parameters such as the spray gun's travel speed, atomization pressure, spray gun flow, nozzle angle, etc. Otherwise, it will lead to poor uniformity of the coating, thereby affecting the performance of the NdFeB material.

[0005] In order to improve the uniformity of spraying, patent CN116140157A discloses a method for spraying the surface of bonded NdFeB magnets, which places the friction object and the NdFeB magnets into a drum, rotates the drum, and then uses a spray gun to spray, so that the friction object can be used to more evenly apply the coating to the surface of the NdFeB magnet; however, when spraying, part of the coating will be sprayed inside the drum, which increases the difficulty of cleaning the drum and the amount of coating, and the coating thickness needs to be tested repeatedly during spraying, which is cumbersome, time-consuming and laborious. Patent CN112076961A rotates the platform on which the NdFeB magnets are placed multiple times, and sprays multiple times to control the thickness accuracy and uniformity of the coating; this method requires multiple spraying, which affects production efficiency. Patent CN109778286A uses a two-step operation of electrophoresis and spraying to replace multiple thickening spraying to obtain a more uniform coating; however, the overall thickness of the coating obtained by this method is relatively large, which is not suitable for the preparation of thin coatings, and the large coating thickness will have a greater impact on the magnetism of the NdFeB magnet.

[0006] In addition to the spraying uniformity of the coating, the bonding strength between the coating and the NdFeB material and the effect of the coating on the magnetism of the NdFeB material are also important factors to be considered in the spraying process. How to ensure the spraying uniformity of the coating, improve the bonding strength of the coating, and weaken the effect of the coating on magnetism without affecting the production efficiency is a key issue that needs to be solved in the production of NdFeB magnets. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a surface spraying process for NdFeB magnets of automotive sensors. The NdFeB magnets are pretreated and the spraying process parameters are adjusted. A coating is prepared on the surface of the NdFeB magnet using a one-time spraying process. The coating has good uniformity, high bonding strength, good corrosion resistance, and little effect on the magnetism of the NdFeB magnet.

[0008] The surface spraying process of the NdFeB magnetic steel for automobile sensors of the present invention comprises the following steps:

[0009] (1) Degreasing and oil removal: Soak the NdFeB magnet in a mixed aqueous solution of sodium carbonate and sodium hydroxide for degreasing and oil removal, and then wash with water;

[0010] (2) Pickling and rust removal: Soak the degreased and deoiled NdFeB magnet in an acid solution for pickling and rust removal, and then wash with water;

[0011] (3) Sealing and filling: Soak the NdFeB magnet after pickling and rust removal in a filling liquid containing polyvinyl alcohol, silane coupling agent, and nano-silicon dioxide for sealing and filling, and then wash with water;

[0012] (4) Air spraying: Place the sealed and filled NdFeB magnets on the spraying platform, and spray both sides with epoxy resin paint diluted with diluent. After spraying the first side, cure it at 160-170℃ for 60-80min. After spraying the second side, cure it at 190-200℃ for 90-120min to obtain a coating with a thickness of 10-15μm.

[0013] In step (1), in the mixed aqueous solution of sodium carbonate and sodium hydroxide, the content of sodium carbonate is 0.5-1.5wt.%, and the content of sodium hydroxide is 0.5-1.5wt.%.

[0014] In step (1), the degreasing time is not less than 20 minutes, and the degreasing can be carried out at room temperature. In order to improve the degreasing efficiency, the degreasing temperature can be increased, but it should not exceed 80°C. Furthermore, ultrasonic treatment can be assisted. The degreasing solution of the present invention does not contain phosphate, thereby reducing the discharge of phosphorus-containing wastewater.

[0015] In step (2), the acid solution is a sulfuric acid solution or a nitric acid solution, and the concentration of the acid solution is not less than 50 wt.%.

[0016] In step (2), the pickling and rust removal time is 20-60s, and the pickling and rust removal can be carried out at room temperature. The rust on the surface of the NdFeB magnet is removed by pickling.

[0017] In step (3), in the filling liquid, the content of polyvinyl alcohol is 5-8wt.%, the content of silane coupling agent is 0.2-0.5wt.%, the content of nano-silicon dioxide is 1-2wt.%, and the balance is water.

[0018] The preparation method of the filling liquid is as follows: completely dissolve polyvinyl alcohol in water at 70-80°C, then add a silane coupling agent, stir evenly, then add nano silicon dioxide, stir until evenly dispersed, and the filling liquid is obtained.

[0019] In step (3), the NdFeB magnet is immersed in the filling liquid for 1-3 minutes, and is immersed 2-3 times. The immersion temperature can be kept at room temperature. In order to improve the sealing filling efficiency, the filling liquid temperature can be appropriately increased, but it should not exceed 40°C.

[0020] During the preparation process, degreasing and oil removal, pickling and rust removal of NdFeB magnets, pores of varying sizes will be formed on the surface of the NdFeB magnets. During air spraying, small pores may be filled by the coating, while depressions will occur where large pores exist, thereby affecting the smoothness of the prepared coating and further affecting the corrosion resistance of the coating. The present invention immerses the NdFeB magnets in a filling liquid, and a silane coupling agent can modify the surface of the NdFeB magnets. Nano-silicon dioxide gathers at the pores on the surface of the NdFeB magnets, and couples with polyvinyl alcohol to achieve a cross-linking effect, thereby sealing and filling the pores.

[0021] In step (4), when stacking the NdFeB magnets, the distance between adjacent NdFeB magnets is 1-1.2 times the height of the NdFeB magnets.

[0022] In step (4), the spraying operation parameters are: the angle between the spray gun and the spraying surface is 45°±1°, the vertical distance between the spray gun and the spraying surface is 12-18 cm, the spray gun travel speed is 20-35 m / min, the spray gun flow rate is 35-40 g / min, and the spray gun atomization pressure is 0.32-0.45 MPa.

[0023] During the spraying process, parameters such as the stacking spacing of NdFeB magnets, spraying angle, spraying distance, spraying speed, spraying flow, atomization pressure, paint viscosity, and curing conditions all affect the uniformity and thickness of the coating. Among them, if the stacking spacing of NdFeB magnets is too large, the number of products sprayed at a single time will be reduced, and the production efficiency will be low. If the stacking spacing is too small, the substrate will be easily exposed on the side of the product or the coating on the side of the product will be too thin. The vertical distance between the spray gun and the spraying surface determines the discrete degree of the paint spray sprayed on the product surface and the coverage range of each spraying. The travel speed of the spray gun determines the time the spray gun stays above the product per unit time during the spraying process. The spray gun flow rate is the mass of the sprayed paint flowing out per minute. These two parameters have a great influence on the coating thickness. The spray gun atomization pressure refers to the air pressure when the paint is dispersed into mist under the action of air pressure, which determines the size of the paint spray particles and ultimately determines the roughness of the coating. The viscosity of the paint affects the smoothness and uniformity of the coating. When the viscosity is too low, the fluidity is too high, which is easy to cause sagging. When the viscosity is too high, the fluidity is too poor, which is easy to cause particle defects. The curing temperature and time have an impact on the curing effect of the coating. If the curing temperature is too low or the time is too short, the coating will become soft and easy to scratch. If the curing temperature is too high or the time is too long, the coating will become brittle and easy to fall off.

[0024] During curing, after the first side is sprayed, the present invention is first cured at a condition slightly lower than the optimal curing temperature, so that the coating is cured to a state that is not soft but not completely cured, and then after the second side is sprayed, it is cured at the optimal curing temperature again. At this time, the coating sprayed on the first side is further cured, so that the coatings on both sides are completely cured at the same time, avoiding the coating sprayed on the first side from being subjected to secondary curing at the optimal curing temperature, which makes the coating brittle and affects the bonding strength and mechanical properties of the coating.

[0025] In step (4), a diluent is added to the epoxy resin coating to adjust its viscosity at 25°C to 0.012-0.013 Pa·s, and then spraying is performed. Preferably, the diluent is a mixture of glutaraldehyde and at least one of n-butanol, ethanol, xylene, and butyl acetate, wherein the mass percentage of glutaraldehyde in the diluent is 0.1-0.5%.

[0026] The present invention adds a diluent to the epoxy resin coating, on the one hand, to adjust the viscosity of the epoxy resin coating to make it moderate so as to obtain a coating with high uniformity and smoothness, and on the other hand, the glutaraldehyde contained in the diluent can undergo a cross-linking reaction with the polyvinyl alcohol remaining in the filling liquid, thereby improving the cross-linking degree of the coating, enhancing the density of the coating, reducing coating defects, and improving the mechanical properties and corrosion resistance of the coating.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention uses a filling liquid containing polyvinyl alcohol, a silane coupling agent, and nano-silicon dioxide to seal and fill the pores of the NdFeB magnet. The silane coupling agent can modify the surface of the NdFeB magnet. The nano-silicon dioxide gathers in the pores on the surface of the NdFeB magnet and couples with the polyvinyl alcohol to achieve a cross-linking effect, thereby sealing and filling the pores. The polyvinyl alcohol remaining in the filling liquid can undergo a cross-linking reaction with the glutaraldehyde contained in the diluent during the spraying process, thereby improving the cross-linking degree of the coating, enhancing the density of the coating, reducing coating defects, and improving the mechanical properties and corrosion resistance of the coating.

[0029] (2) In the spraying process, the present invention optimizes the NdFeB magnet stacking spacing, spraying angle, spraying distance, spraying speed, spraying flow, atomization pressure, coating viscosity, curing conditions and other parameters, so that a coating with good uniformity, high smoothness and appropriate thickness can be obtained by spraying once, and the production efficiency is high;

[0030] (3) During curing, after spraying the first side, the present invention first cures at a temperature slightly lower than the optimal curing temperature, so that the coating is cured to a state where it is not soft but not completely cured. After spraying the second side, the coating is cured at the optimal curing temperature again. At this time, the coating sprayed on the first side is further cured, so that the coatings on both sides are completely cured at the same time, thereby avoiding the coating sprayed on the first side from being subjected to secondary curing at the optimal curing temperature, which causes the coating to become brittle and affects the bonding strength and mechanical properties of the coating.

[0031] (4) The coating thickness prepared by the present invention is 10-15 μm, which is much lower than the thickness of the epoxy resin coating in the prior art. On the one hand, the smaller coating thickness has less effect on the magnetism of the NdFeB magnet. On the other hand, the present invention improves the pretreatment process and spraying process of the NdFeB magnet, so that the coating has the same excellent bonding strength and corrosion resistance at a lower thickness. DETAILED DESCRIPTION

[0032] The technical scheme of the present invention is further described below in conjunction with the examples. Unless otherwise specified, all raw materials used in the examples are commercially available.

[0033] Example 1

[0034] A surface spraying process for NdFeB magnetic steel of automobile sensors, comprising the following steps:

[0035] (1) Degreasing and oil removal: Soak the NdFeB magnet in a mixed aqueous solution of 1wt.% sodium carbonate and 1wt.% sodium hydroxide for 20 minutes for degreasing and oil removal, and then wash with water;

[0036] (2) Pickling and rust removal: Soak the degreased and deoiled NdFeB magnet in a 60wt.% sulfuric acid solution for 20s for pickling and rust removal, and then wash with water;

[0037] (3) Sealing and filling: prepare a filling liquid with a polyvinyl alcohol content of 6wt.%, a silane coupling agent KH-560 content of 0.3wt.%, and a nano-silica content of 1.5wt.%, and completely dissolve the polyvinyl alcohol in 70°C water, then add the silane coupling agent KH-560, stir evenly, then add the nano-silica, and stir until evenly dispersed.

[0038] Soak the pickled and rust-removed NdFeB magnet in the above filling liquid for 2 minutes, take it out and drain it, soak it again for 2 minutes, repeat the operation 3 times, seal the holes, and then wash it with water;

[0039] (4) Air spraying: Place the sealed and filled NdFeB magnets on the spraying platform, with the distance between adjacent NdFeB magnets being 1 times the height of the NdFeB magnets. Use a mixed diluent of n-butanol and glutaraldehyde (the mass percentage of glutaraldehyde is 0.3%) to dilute the epoxy resin coating to a viscosity of 0.012 Pa·s at 25°C, and then spray it. The spraying operating parameters are as follows: the angle between the spray gun and the spraying surface is 45°±1°, the vertical distance between the spray gun and the spraying surface is 15 cm, the spray gun travel speed is 30 m / min, the spray gun flow rate is 38 g / min, and the spray gun atomization pressure is 0.4 MPa. After the first side is sprayed, it is cured at 160°C for 80 min. After the second side is sprayed, it is cured at 190°C for 120 min to obtain a coating with a thickness of 12 μm.

[0040] Example 2

[0041] A surface spraying process for NdFeB magnetic steel of automobile sensors, comprising the following steps:

[0042] (1) Degreasing and oil removal: Soak the NdFeB magnet in a mixed aqueous solution of 0.5wt.% sodium carbonate and 1.5wt.% sodium hydroxide for 25 minutes for degreasing and oil removal, and then wash with water;

[0043] (2) Pickling and rust removal: Soak the degreased and deoiled NdFeB magnet in 65wt.% nitric acid solution for 40s for pickling and rust removal, and then wash with water;

[0044] (3) Sealing and filling: prepare a filling liquid with a polyvinyl alcohol content of 8wt.%, a silane coupling agent KH-560 content of 0.5wt.%, and a nano-silica content of 2wt.%, and completely dissolve the polyvinyl alcohol in 80°C water. Then add the silane coupling agent KH-560, stir evenly, and then add the nano-silica. Stir until it is evenly dispersed.

[0045] Soak the pickled and rust-removed NdFeB magnet in the above filling liquid for 1 minute, take it out and drain it, soak it again for 1 minute, repeat the operation 3 times, seal the holes, and then wash it with water;

[0046] (4) Air spraying: Place the sealed and filled NdFeB magnets on the spraying platform, with the distance between adjacent NdFeB magnets being 1 times the height of the NdFeB magnets. Use a mixed diluent of butyl acetate and glutaraldehyde (the mass percentage of glutaraldehyde is 0.1%) to dilute the epoxy resin coating to a viscosity of 0.012 Pa·s at 25°C, and then spray it. The spraying operating parameters are: the angle between the spray gun and the spraying surface is 45°±1°, the vertical distance between the spray gun and the spraying surface is 18 cm, the spray gun travel speed is 20 m / min, the spray gun flow rate is 35 g / min, and the spray gun atomization pressure is 0.45 MPa. After the first side is sprayed, it is cured at 165°C for 90 min. After the second side is sprayed, it is cured at 195°C for 100 min to obtain a coating with a thickness of 10 μm.

[0047] Example 3

[0048] A surface spraying process for NdFeB magnetic steel of automobile sensors, comprising the following steps:

[0049] (1) Degreasing and oil removal: Soak the NdFeB magnet in a mixed aqueous solution of 1.5wt.% sodium carbonate and 0.5wt.% sodium hydroxide for 30 minutes for degreasing and oil removal, and then wash with water;

[0050] (2) Pickling and rust removal: Soak the degreased and deoiled NdFeB magnet in a 50wt.% sulfuric acid solution for 60s for pickling and rust removal, and then wash with water;

[0051] (3) Sealing and filling: prepare a filling liquid with a polyvinyl alcohol content of 5wt.%, a silane coupling agent KH-560 content of 0.2wt.%, and a nano-silica content of 1wt.%, and completely dissolve the polyvinyl alcohol in 75°C water. Then add the silane coupling agent KH-560, stir evenly, and then add the nano-silica. Stir until it is evenly dispersed.

[0052] Soak the pickled and rust-removed NdFeB magnet in the above filling liquid for 3 minutes, take it out and drain it, soak it again for 3 minutes, repeat the operation twice, seal the holes, and then wash it with water;

[0053] (4) Air spraying: Place the sealed and filled NdFeB magnets on the spraying platform, with the distance between adjacent NdFeB magnets being 1.2 times the height of the NdFeB magnets. Use a mixed diluent of xylene and glutaraldehyde (the mass percentage of glutaraldehyde is 0.5%) to dilute the epoxy resin coating to a viscosity of 0.013 Pa·s at 25°C, and then spray it. The spraying operating parameters are as follows: the angle between the spray gun and the spraying surface is 45°±1°, the vertical distance between the spray gun and the spraying surface is 12 cm, the spray gun travel speed is 35 m / min, the spray gun flow rate is 40 g / min, and the spray gun atomization pressure is 0.32 MPa. After the first side is sprayed, it is cured at 170°C for 60 min. After the second side is sprayed, it is cured at 200°C for 90 min to obtain a coating with a thickness of 15 μm.

[0054] Comparative Example 1

[0055] The difference between this comparative example and Example 1 is that the hole sealing filling in step (3) is not performed, and the NdFeB magnet after pickling and rust removal is directly air sprayed.

[0056] Comparative Example 2

[0057] The only difference between this comparative example and Example 1 is that glutaraldehyde is not added to the diluent in step (4).

[0058] Comparative Example 3

[0059] The only difference between this comparative example and Example 1 is that after the first surface is sprayed in step (4), it is cured at 190° C. for 120 min.

[0060] The coating obtained after the surface spraying of each embodiment and comparative example was tested for coating adhesion, corrosion resistance and magnetic properties. The test method is as follows: the coating adhesion is tested with reference to the standard GB / T 9286-1998, using the hundred-grid test method, that is, using a hundred-grid knife and a hundred-grid board to draw uniform grid lines on the coating, and then using a hundred-grid test special tape to stick to the coating surface. When the tape is torn off without the coating falling off, it is qualified, and if the coating falls off, it is unqualified; the corrosion resistance is measured by salt spray resistance time, and the test is measured with reference to the standard GB / T 1771-1991, and the test conditions are sodium chloride concentration 5wt.%, temperature 35°C; the magnetic property is measured by thermal demagnetization rate, and the thermal demagnetization experimental conditions are 150°C×2h, open circuit. The test results are shown in Table 1.

[0061] Table 1 Test results of coating properties of various embodiments and comparative examples

[0062] project Binding force Salt spray resistance time, h Thermal demagnetization rate, % Appearance Example 1 All sprayed surfaces are qualified >360 1.2 Smooth and even Example 2 All sprayed surfaces are qualified >360 0.9 Smooth and even Example 3 All sprayed surfaces are qualified >360 1.4 Smooth and even Comparative Example 1 All sprayed surfaces failed 92 1.1 There are pits, not smooth Comparative Example 2 A small number of sprayed surfaces are unqualified 240 1.2 Smooth and even Comparative Example 3 Most of the sprayed surfaces are unqualified 45 1.1 Part of the topcoat is cracked

[0063] As can be seen from Table 1, the coating obtained by the spraying process of the present invention has a smooth and uniform appearance, high bonding strength with the substrate, long salt spray resistance time, and low thermal demagnetization rate. Comparative Example 1 does not perform pore sealing and filling, and the obtained coating has pits, is not smooth, has poor bonding strength with the substrate, and has a shortened salt spray resistance time; Comparative Example 2 does not add glutaraldehyde to the diluent, and the bonding strength between the coating and the substrate is slightly reduced, and the salt spray resistance time is shortened; After the two-sided spraying of Comparative Example 3 is completed, curing is performed under the same conditions, resulting in the coating obtained by spraying on the first side being cured twice, resulting in part of the coating simply cracking, reduced bonding strength with the substrate, and greatly shortened salt spray resistance time. In addition, under the condition of substantially the same coating thickness as that of the present invention, since the coating defects of comparative examples 1-3 are relatively more, the effect on the magnetism of NdFeB magnets is relatively small, so the thermal demagnetization rate is slightly lower than that of the present invention; in practical applications, the coating thickness is generally increased by increasing the number of spraying times or superimposing other film layers to eliminate coating defects, but the increase in coating thickness will lead to an increase in thermal demagnetization rate. The present invention reduces the coating thickness on the basis of ensuring the corrosion resistance and uniformity of the coating, thereby reducing the thermal demagnetization rate.

Claims

1. A surface spraying process for NdFeB magnets of automotive sensors, characterized by: The following steps are involved: (1) Degreasing and oil removal: Soak the NdFeB magnet in a mixed aqueous solution of sodium carbonate and sodium hydroxide for degreasing and oil removal, and then wash with water; (2) Pickling and rust removal: Soak the degreased and deoiled NdFeB magnet in an acid solution for pickling and rust removal, and then wash with water; (3) Sealing and filling: Soak the NdFeB magnet after pickling and rust removal in a filling liquid containing polyvinyl alcohol, silane coupling agent, and nano-silicon dioxide for sealing and filling, and then wash with water; (4) Air spraying: Place the sealed and filled NdFeB magnets on the spraying platform, and spray both sides with epoxy resin paint diluted with diluent. After spraying the first side, cure it at 160-170℃ for 60-80min, and after spraying the second side, cure it at 190-200℃ for 90-120min to obtain a coating with a thickness of 10-15μm. In step (3), in the filling liquid, the content of polyvinyl alcohol is 5-8wt.%, the content of silane coupling agent is 0.2-0.5wt.%, the content of nano-silicon dioxide is 1-2wt.%, and the balance is water; In step (4), the diluent is a mixture of at least one of n-butanol, ethanol, xylene, and butyl acetate and glutaraldehyde, wherein the mass percentage of glutaraldehyde in the diluent is 0.1-0.5%.

2. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1 is characterized in that: In step (1), in the mixed aqueous solution of sodium carbonate and sodium hydroxide, the content of sodium carbonate is 0.5-1.5wt.%, and the content of sodium hydroxide is 0.5-1.5wt.%.

3. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1 is characterized in that: In step (2), the acid solution is a sulfuric acid solution or a nitric acid solution, and the concentration of the acid solution is not less than 50wt.%.

4. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1 is characterized in that: In step (2), the pickling and rust removal time is 20-60s.

5. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1 is characterized in that: In step (3), the NdFeB magnet is immersed in the filling liquid for 1-3 minutes, and is immersed 2-3 times.

6. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1 is characterized in that: In step (4), when stacking the NdFeB magnets, the distance between adjacent NdFeB magnets is 1-1.2 times the height of the NdFeB magnets.

7. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1 is characterized by: In step (4), the spraying operation parameters are: the angle between the spray gun and the spraying surface is 45°±1°, the vertical distance between the spray gun and the spraying surface is 12-18 cm, the spray gun travel speed is 20-35 m / min, the spray gun flow rate is 35-40 g / min, and the spray gun atomization pressure is 0.32-0.45 MPa.

8. The surface spraying process of NdFeB magnet for automobile sensor according to claim 1, characterized in that: In step (4), a diluent is added to the epoxy resin coating to adjust its viscosity at 25° C. to 0.012-0.013 Pa·s before spraying.