Stripping liquid suitable for flexible circuit board and preparation method thereof

By using the film stripping liquid with synergistic effect of nitro, hydroxyl and amide groups in the film stripping liquid, the problems of dry film residue and square resistance in the flexible circuit board are solved, and efficient peeling and circuitry are achieved The plate protection improves the speed and efficiency of film stripping, and is environmentally friendly.

CN118530786BActive Publication Date: 2024-11-15SHENZHEN TIANXI SCI DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410596101.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-14
Publication Date
2024-11-15
Estimated Expiration
2044-05-14

AI Technical Summary

Technical Problem

In the processing of flexible circuit boards, traditional film stripping liquid has problems such as dry film residue, slow film stripping speed, large metal attacks, winding rollers and plugging nozzles, and the impact on the square resistance of the circuit board cannot be effectively solved.

Method used

The defiling agent is phthalimide derivative, the inorganic base is strontium hydroxide, the organic base is ethylenediamine, the surfactant is nonylphenol polyoxyethylene ether and octadecyl trimethyl bromide The film stripping liquid of ammonium dioxide achieves efficient peeling of dry films and protection of circuit boards through the synergistic action of nitro, hydroxyl and amide groups.

Benefits of technology

It achieves good peeling of dry film in flexible circuit board without residue, reduces the impact on the circuit board square resistance, improves the film stripping speed and efficiency, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a film stripping solution suitable for a flexible circuit board and a preparation method thereof, and belongs to the field of printed circuit board film stripping technology. The film stripping solution suitable for a flexible circuit board is composed of the following raw materials in mass percentage: 25-40wt% of a film stripping agent, 10-20wt% of an inorganic base, 3-8wt% of an organic base, 5-12wt% of a surfactant, 3-6wt% of an auxiliary agent, and the remainder is a solvent. The film stripping agent used in the present invention has good properties, and the present invention adds a phthalimide derivative that has a different effect on the stripping of the interlayer, has a good stripping effect on the "dry film" in the circuit board, and has a very small effect on the square resistance of the circuit board, does not cause damage to the circuit board, has very little corrosiveness, and is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuit board stripping, and in particular to a stripping liquid suitable for a flexible circuit board and a preparation method thereof. Background Art

[0002] Flexible circuit boards are the main components of electronic products. The average use time of components on waste circuit boards is about 20,000 hours, which is still at the best quality period. After electrical performance testing and targeted repairs, they can still be reused in electronic product production. However, due to the complexity of the production process, scratches, stains, warping and other defects may appear on the surface of flexible circuit boards, affecting the function and reliability of the circuit boards.

[0003] In the process of preparing circuit boards, whether the anti-etching film can be completely removed after etching directly affects the progress of the subsequent process and the quality of the circuit boards. Therefore, the film stripping process is a key process in the process of preparing circuit boards. At present, sodium hydroxide solution is generally used as the film stripping solution. The chemical oxygen demand of the waste liquid generated after the film stripping treatment is high, and the cost of post-treatment of the waste liquid is high.

[0004] Traditional stripping liquid is mainly made of sodium hydroxide, which can no longer meet the requirements of stripping ultra-fine circuits in the circuit board industry. Traditional stripping liquid cannot crush the extremely narrow dry film required for micro-fineness, and it is easy to produce dry film residue, which is what we call "film sandwich". The main reason for "film sandwich" is that water molecules and the main components of the stripping agent are absorbed into the dry film, causing the dry film to expand. The expanded dry film is firmly sandwiched between the circuits. Because the circuit spacing is very small, the expanded dry film is tightly sandwiched between the line spacing, and the stripping agent cannot continue to penetrate, causing the dry film to be unable to crack and fall off from the circuit. Film sandwich will cause problems such as product short circuits, reduced conductivity or even scrapping, and increased production costs. In addition, traditional stripping liquids also have disadvantages such as slow stripping speed, metal attack, large film scraps wrapping around the roller, and easy nozzle clogging. Therefore, it is necessary to improve the existing stripping liquid.

[0005] Chinese invention patent CN 113563888 A discloses a stripping solution and its preparation method. The stripping solution components include 30%-45% of composite alkali, 20%-30% of surfactant, 5%-9% of corrosion inhibitor, and the rest is water. Although the stripping solution prepared by the invention can improve the stripping treatment effect, the invention does not effectively solve the problem of how the square resistance of the circuit board will be affected after the treatment. Will it affect the subsequent use? In view of this shortcoming, the present invention designs a stripping solution that is environmentally friendly and has very low corrosiveness to the circuit board. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a stripping solution suitable for flexible circuit boards and a preparation method thereof.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0008] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 25-40wt% of a film stripping agent, 10-20wt% of an inorganic base, 3-8wt% of an organic base, 5-12wt% of a surfactant, 3-6wt% of an auxiliary agent, and the balance being a solvent.

[0009] The demolding agent is at least one of phthalimidoglutaric acid, 3-phthalimidopropionic acid, N-hydroxy-4-nitrophthalimide or phthalimide derivatives.

[0010] Phthalimide derivatives are closer to some specific components of the dry film. When they are combined with organic bases and inorganic bases in a certain proportion, the stripping of the dry film is more in line with the principle of "like dissolves like" and is more conducive to the stripping of ultra-fine circuits.

[0011] The preparation method of the phthalimide derivative comprises the following steps:

[0012] S1, 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate react in 1,2-dichloroethane and trimethylsilyl trifluoromethanesulfonate to obtain intermediate I; 1,6-heptadien-4-ol is added to the obtained intermediate I to react to obtain intermediate II; sodium periodate and water are added to the obtained intermediate II to react in the presence of a catalyst, ruthenium trichloride, to obtain carboxyl-modified N-acetamidogalactose;

[0013] S2, N-hydroxy-4-nitrophthalimide and the above-mentioned carboxyl-modified N-acetamidogalactose are reacted to obtain a phthalimide derivative.

[0014] The reaction mechanism of the present invention is as follows: First, in S1, 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate undergoes an intramolecular reaction under the conditions of trimethylsilyl trifluoromethanesulfonate, and the acetate group and the acetylamino group undergo an addition reaction to obtain an intermediate I ; 1,6-heptadien-4-ol is then added to react under stirring to cause an addition reaction, thereby opening the ring N=CO in the intermediate I and introducing a C=C double bond. In the presence of periodic acid and a catalyst, ruthenium trichloride, the C=C double bond is oxidized to -COOH to obtain carboxyl-modified N-acetamidogalactose containing -COOH; N-hydroxy-4-nitrophthalimide is then added to form an amide bond under the catalysis of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate to finally obtain a phthalimide derivative. The phthalimide derivative prepared by the present invention contains effective groups such as nitro, hydroxyl and amide.

[0015] Preferably, the preparation method of the phthalimide derivative comprises the following steps:

[0016] S1. In an ice-water bath and under nitrogen protection, 3-6 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, 20-50 parts by weight of 1,2-dichloroethane, and 1-3 parts by weight of trimethylsilyl trifluoromethanesulfonate are mixed, stirred at 30-45° C. and 400-800 rpm for 6-20 hours, and then 30-60 parts by weight of saturated sodium carbonate aqueous solution are added and stirred for 30-60 minutes, and the mixture is extracted, separated, washed, and distilled under reduced pressure to obtain an intermediate I; 18-30 parts by weight of 1,2-dichloroethane and 1-4 parts by weight of 1,6-heptadien-4-ol are added to the obtained intermediate I, and stirred at 30-45° C. and 400-800 rpm for 10-30 minutes, and then 1-3 parts by weight of trimethylsilyl trifluoromethanesulfonate are added. trimethylsilyl fluoromethanesulfonate, continue stirring for 5-20h, then add 30-60 parts by weight of saturated sodium carbonate aqueous solution and continue stirring for 30-60min, extract and separate, wash, and distill under reduced pressure to obtain intermediate II; add 20-40 parts by weight of dichloromethane and 20-40 parts by weight of acetonitrile as a mixed solvent to the obtained intermediate II, then add 20-50 parts by weight of water and 3-6 parts by weight of sodium periodate, stir at room temperature and 400-800rpm for 8-20min, add 0.05-0.2 parts by weight of ruthenium trichloride, stir at 30-45°C and 400-800rpm for 5-20h, add 30-60 parts by weight of water and stir, adjust the pH to 7.5, extract and separate, wash, and distill under reduced pressure to obtain carboxyl-modified N-acetamidogalactose;

[0017] S2. Mix 0.5-2 parts by weight of N-hydroxy-4-nitrophthalimide, 1-3 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 20-60 parts by weight of N,N-dimethylformamide, add 1-3 parts by weight of the above-mentioned carboxyl-modified N-acetamidogalactose, stir at room temperature and 200-600 rpm for 3-6 hours, extract and separate, wash, and distill under reduced pressure. Dissolve the obtained product in 5-10 parts by weight of methanol and 0.5-3 parts by weight of triethylamine, react at 45-55° C. for 16-36 hours, and distill under reduced pressure to remove the solvent to obtain a phthalimide derivative.

[0018] The phthalimide derivatives prepared by the present invention contain nitro, hydroxyl and amide groups, which play different roles in the stripping of the interlayer in the film stripping solution: the nitro group enhances the organic solubility of the phthalimide derivatives, making it more effective in dissolving the adhesive or glue; the presence of the nitro group increases the polarity of the molecule and improves its solubility in organic solvents, thereby promoting the dissolution and stripping of the adhesive. The hydroxyl group increases the surface activity of the phthalimide derivatives, making it easier to form hydrogen bonds or other interactions with the surface of the circuit board, enhancing the contact between the film stripping solution and the interlayer, which helps to improve the stripping efficiency and speed; the hydroxyl group undergoes a hydrolysis reaction with specific components in the interlayer, destroying the structure of the adhesive and leading to the stripping of the interlayer material, and this hydrolysis can accelerate the separation process of the film stripping solution and the interlayer; it participates in the chemical reaction between the film stripping solution and the specific components in the interlayer, accelerating the film stripping process, thereby achieving the stripping of the interlayer. The amide group gives phthalimide derivatives the ability to selectively strip specific types of adhesives, which means that they can strip specific components in the circuit board without damaging other materials, thereby ensuring the integrity and quality of the circuit board and reducing the impact on the square resistance of the circuit board.

[0019] In summary, the nitro, hydroxyl and amide groups in phthalimide derivatives have different stripping effects on the interlayer in the stripping solution, including dissolution, surface activity, hydrolysis and selectivity, which play a comprehensive role in accelerating the stripping process.

[0020] The inorganic base is at least one of sodium hydroxide, barium hydroxide, calcium hydroxide and strontium hydroxide; preferably, the inorganic base is strontium hydroxide.

[0021] Strontium hydroxide solution is usually milder in alkalinity than sodium hydroxide solution. During use, strontium hydroxide can reduce corrosion and damage to substrates and other materials, reduce unnecessary damage or incomplete stripping, and has a better selective stripping effect on specific types of adhesives or resins. Strontium hydroxide may be more environmentally friendly than sodium hydroxide, and thus can be used more safely in the circuit board manufacturing process.

[0022] The organic base is at least one of ethylenediamine, sodium ethoxide, triethylamine, triethylenetetramine, and tetramethylammonium hydroxide.

[0023] Organic bases can act as ligands in the stripping solution to form a complex with the copper surface. This complex helps to improve the wettability of the stripping solution on the copper surface, thereby promoting the contact between the stripping solution and the circuit board. It can also improve the solubility of the stripping solution in some difficult-to-dissolve materials and improve the stripping efficiency. The alkalinity of organic bases is very mild and has a strong selective stripping effect on specific types of adhesives or resins. It can specifically strip the target film without damaging other materials.

[0024] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyl trimethyl bromide.

[0025] Surfactants can increase the contact area between the stripping solution and the film and improve the stripping efficiency. Nonylphenol polyoxyethylene ether may be used as a nonionic surfactant, while octadecyl trimethyl ammonium bromide may be used as a cationic surfactant. The two can work together to improve the wettability of the stripping solution.

[0026] The auxiliary agent is any one of α-bromo-p-hydroxyacetophenone and 2-fluoro-6-hydroxyacetophenone; preferably, the auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0027] 2-Fluoro-6-hydroxyacetophenone can reduce the possibility of the film attaching to the substrate again after stripping by forming a thin film or changing the surface energy, which helps to improve the wettability and surface tension adjustment ability of the stripping solution, which helps the stripper to be more evenly distributed on the surface of the circuit board, improve the stability of the stripping solution, prevent the stripping solution from changing or decomposing during use, and accelerate the contact between the stripping solution and the film, thereby improving the stripping efficiency.

[0028] The solvent is a mixture of water and diethylene glycol monobutyl ether.

[0029] The method for preparing a film stripping liquid suitable for a flexible circuit board comprises the following steps: mixing a film stripping agent, an inorganic base, an organic base, a surfactant, an auxiliary agent and a solvent, and stirring them evenly to obtain a film stripping liquid suitable for a flexible circuit board.

[0030] Beneficial effects of the invention: The invention provides a stripping liquid suitable for a flexible circuit board and a preparation method thereof. Phthalimide derivatives having different effects on the stripping of the interlayer are added to the raw materials of the stripping liquid. The stripping liquid has a good stripping effect on the "dry film" in the circuit board, and the treatment is clean and residue-free. At the same time, the effect on the square resistance of the circuit board is very small. The stripping liquid for the flexible circuit board prepared by the invention has a good stripping effect on the "interlayer", does not damage the circuit board, has little corrosiveness, and is environmentally friendly. DETAILED DESCRIPTION

[0031] The above content of the present invention is further described in detail below in conjunction with specific implementation modes, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments.

[0032] Introduction of some raw materials in this application:

[0033] 2-(Acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, CAS: 3006-60-8.

[0034] Nonylphenol polyoxyethylene ether was purchased from Shandong Xiangzhao New Materials Co., Ltd., model: np-10.

[0035] Example 1

[0036] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 30wt% of a film stripping agent, 15wt% of an inorganic base, 5wt% of an organic base, 10wt% of a surfactant, 5wt% of an auxiliary agent, and the balance being a solvent.

[0037] The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps:

[0038] S1. In an ice-water bath and under nitrogen protection, 4 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, 25 parts by weight of 1,2-dichloroethane, and 2 parts by weight of trimethylsilyl trifluoromethanesulfonate were mixed, stirred at 35° C. and 600 rpm for 8 hours, and then 40 parts by weight of saturated sodium carbonate aqueous solution were added and stirred for 40 minutes, and the mixture was extracted, separated, washed, and distilled under reduced pressure to obtain intermediate I; 20 parts by weight of 1,2-dichloroethane and 2 parts by weight of 1,6-heptadien-4-ol were added to the obtained intermediate I, and stirred at 35° C. and 600 rpm for 20 minutes, and then 2 parts by weight of saturated sodium carbonate aqueous solution were added. trimethylsilyl trifluoromethanesulfonate, continue stirring for 10 hours, then add 40 parts by weight of saturated sodium carbonate aqueous solution and continue stirring for 40 minutes, extract and separate, wash, and distill under reduced pressure to obtain intermediate II; add 25 parts by weight of dichloromethane and 25 parts by weight of acetonitrile as a mixed solvent to the obtained intermediate II, then add 30 parts by weight of water and 4 parts by weight of sodium periodate, stir at room temperature and 600 rpm for 10 minutes, add 0.1 parts by weight of ruthenium trichloride, stir at 35°C and 600 rpm for 10 hours, add 40 parts by weight of water and stir, adjust the pH to 7.5, extract and separate, wash, and distill under reduced pressure to obtain carboxyl-modified N-acetamidogalactose;

[0039] S2. Mix 1 part by weight of N-hydroxy-4-nitrophthalimide, 2 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 30 parts by weight of N,N-dimethylformamide, add 2 parts by weight of the above-mentioned carboxyl-modified N-acetamidogalactose, stir at room temperature and 400 rpm for 4 hours, extract and separate the liquids, wash, and distill under reduced pressure. Dissolve the obtained product in 8 parts by weight of methanol and 1 part by weight of triethylamine, react at 50°C for 24 hours, and remove the solvent by distillation under reduced pressure to obtain a phthalimide derivative.

[0040] The inorganic base is strontium hydroxide.

[0041] The organic base is ethylenediamine.

[0042] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0043] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0044] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0045] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 30 wt% of a stripping agent, 15 wt% of strontium hydroxide, 5 wt% of ethylenediamine, 10 wt% of a surfactant, 5 wt% of 2-fluoro-6-hydroxyacetophenone and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0046] Example 2

[0047] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 25wt% of a film stripping agent, 20wt% of an inorganic base, 3wt% of an organic base, 12wt% of a surfactant, 3wt% of an auxiliary agent, and the balance being a solvent.

[0048] The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps:

[0049] S1. In an ice-water bath and under nitrogen protection, 4 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, 25 parts by weight of 1,2-dichloroethane, and 2 parts by weight of trimethylsilyl trifluoromethanesulfonate were mixed, stirred at 35° C. and 600 rpm for 8 hours, and then 40 parts by weight of saturated sodium carbonate aqueous solution were added and stirred for 40 minutes, and the mixture was extracted, separated, washed, and distilled under reduced pressure to obtain intermediate I; 20 parts by weight of 1,2-dichloroethane and 2 parts by weight of 1,6-heptadien-4-ol were added to the obtained intermediate I, and stirred at 35° C. and 600 rpm for 20 minutes, and then 2 parts by weight of saturated sodium carbonate aqueous solution were added. trimethylsilyl trifluoromethanesulfonate, continue stirring for 10 hours, then add 40 parts by weight of saturated sodium carbonate aqueous solution and continue stirring for 40 minutes, extract and separate, wash, and distill under reduced pressure to obtain intermediate II; add 25 parts by weight of dichloromethane and 25 parts by weight of acetonitrile as a mixed solvent to the obtained intermediate II, then add 30 parts by weight of water and 4 parts by weight of sodium periodate, stir at room temperature and 600 rpm for 10 minutes, add 0.1 parts by weight of ruthenium trichloride, stir at 35°C and 600 rpm for 10 hours, add 40 parts by weight of water and stir, adjust the pH to 7.5, extract and separate, wash, and distill under reduced pressure to obtain carboxyl-modified N-acetamidogalactose;

[0050] S2. Mix 1 part by weight of N-hydroxy-4-nitrophthalimide, 2 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 30 parts by weight of N,N-dimethylformamide, add 2 parts by weight of the above-mentioned carboxyl-modified N-acetamidogalactose, stir at room temperature and 400 rpm for 4 hours, extract and separate the liquids, wash, and distill under reduced pressure. Dissolve the obtained product in 8 parts by weight of methanol and 1 part by weight of triethylamine, react at 50°C for 24 hours, and remove the solvent by distillation under reduced pressure to obtain a phthalimide derivative.

[0051] The inorganic base is strontium hydroxide.

[0052] The organic base is ethylenediamine.

[0053] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0054] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0055] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0056] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 25wt% of a stripping agent, 20wt% of an inorganic base, 3wt% of an organic base, 12wt% of a surfactant, 3wt% of 2-fluoro-6-hydroxyacetophenone, and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0057] Example 3

[0058] A film stripping solution suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 40wt% of a film stripping agent, 10wt% of an inorganic base, 8wt% of an organic base, 5wt% of a surfactant, 6wt% of an auxiliary agent, and the balance being a solvent.

[0059] The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps:

[0060] S1. In an ice-water bath and under nitrogen protection, 4 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, 25 parts by weight of 1,2-dichloroethane, and 2 parts by weight of trimethylsilyl trifluoromethanesulfonate were mixed, stirred at 35° C. and 600 rpm for 8 hours, and then 40 parts by weight of saturated sodium carbonate aqueous solution were added and stirred for 40 minutes, and the mixture was extracted, separated, washed, and distilled under reduced pressure to obtain intermediate I; 20 parts by weight of 1,2-dichloroethane and 2 parts by weight of 1,6-heptadien-4-ol were added to the obtained intermediate I, and stirred at 35° C. and 600 rpm for 20 minutes, and then 2 parts by weight of saturated sodium carbonate aqueous solution were added. trimethylsilyl trifluoromethanesulfonate, continue stirring for 10 hours, then add 40 parts by weight of saturated sodium carbonate aqueous solution and continue stirring for 40 minutes, extract and separate, wash, and distill under reduced pressure to obtain intermediate II; add 25 parts by weight of dichloromethane and 25 parts by weight of acetonitrile as a mixed solvent to the obtained intermediate II, then add 30 parts by weight of water and 4 parts by weight of sodium periodate, stir at room temperature and 600 rpm for 10 minutes, add 0.1 parts by weight of ruthenium trichloride, stir at 35°C and 600 rpm for 10 hours, add 40 parts by weight of water and stir, adjust the pH to 7.5, extract and separate, wash, and distill under reduced pressure to obtain carboxyl-modified N-acetamidogalactose;

[0061] S2. Mix 1 part by weight of N-hydroxy-4-nitrophthalimide, 2 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 30 parts by weight of N,N-dimethylformamide, add 2 parts by weight of the above-mentioned carboxyl-modified N-acetamidogalactose, stir at room temperature and 400 rpm for 4 hours, extract and separate the liquids, wash, and distill under reduced pressure. Dissolve the obtained product in 8 parts by weight of methanol and 1 part by weight of triethylamine, react at 50°C for 24 hours, and remove the solvent by distillation under reduced pressure to obtain a phthalimide derivative.

[0062] The inorganic base is strontium hydroxide.

[0063] The organic base is ethylenediamine.

[0064] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0065] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0066] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0067] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 40 wt% of a stripping agent, 10 wt% of an inorganic base, 8 wt% of an organic base, 5 wt% of a surfactant, 6 wt% of 2-fluoro-6-hydroxyacetophenone and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0068] Comparative Example 1

[0069] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 30wt% of a film stripping agent, 15wt% of an inorganic base, 5wt% of an organic base, 10wt% of a surfactant, 5wt% of an auxiliary agent, and the balance being a solvent.

[0070] The demoulding agent is N-hydroxy-4-nitrophthalimide.

[0071] The inorganic base is strontium hydroxide.

[0072] The organic base is ethylenediamine.

[0073] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0074] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0075] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0076] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 30 wt% of a stripping agent, 15 wt% of strontium hydroxide, 5 wt% of ethylenediamine, 10 wt% of a surfactant, 5 wt% of 2-fluoro-6-hydroxyacetophenone and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0077] Comparative Example 2

[0078] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 30wt% of a film stripping agent, 15wt% of an inorganic base, 5wt% of an organic base, 10wt% of a surfactant, 5wt% of an auxiliary agent, and the balance being a solvent.

[0079] The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps:

[0080] S1. In an ice-water bath and under nitrogen protection, 4 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, 25 parts by weight of 1,2-dichloroethane, and 2 parts by weight of trimethylsilyl trifluoromethanesulfonate were mixed, stirred at 35° C. and 600 rpm for 8 hours, and then 40 parts by weight of saturated sodium carbonate aqueous solution were added and stirred for 40 minutes, and the mixture was extracted, separated, washed, and distilled under reduced pressure to obtain intermediate I; 20 parts by weight of 1,2-dichloroethane and 2 parts by weight of 1,6-heptadien-4-ol were added to the obtained intermediate I, and stirred at 35° C. and 600 rpm for 20 minutes, and then 2 parts by weight of saturated sodium carbonate aqueous solution were added. trimethylsilyl trifluoromethanesulfonate, continue stirring for 10 hours, then add 40 parts by weight of saturated sodium carbonate aqueous solution and continue stirring for 40 minutes, extract and separate, wash, and distill under reduced pressure to obtain intermediate II; add 25 parts by weight of dichloromethane and 25 parts by weight of acetonitrile as a mixed solvent to the obtained intermediate II, then add 30 parts by weight of water and 4 parts by weight of sodium periodate, stir at room temperature and 600 rpm for 10 minutes, add 0.1 parts by weight of ruthenium trichloride, stir at 35°C and 600 rpm for 10 hours, add 40 parts by weight of water and stir, adjust the pH to 7.5, extract and separate, wash, and distill under reduced pressure to obtain carboxyl-modified N-acetamidogalactose;

[0081] S2. Mix 1 part by weight of N-hydroxy-4-nitrophthalimide, 2 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 30 parts by weight of N,N-dimethylformamide, add 2 parts by weight of the above-mentioned carboxyl-modified N-acetamidogalactose, stir at room temperature and 400 rpm for 4 hours, extract and separate the liquids, wash, and distill under reduced pressure. Dissolve the obtained product in 8 parts by weight of methanol and 1 part by weight of triethylamine, react at 50°C for 24 hours, and remove the solvent by distillation under reduced pressure to obtain a phthalimide derivative.

[0082] The inorganic base is sodium hydroxide.

[0083] The organic base is ethylenediamine.

[0084] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0085] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0086] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0087] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 30wt% of a stripping agent, 15wt% of sodium hydroxide, 5wt% of ethylenediamine, 10wt% of a surfactant, 5wt% of 2-fluoro-6-hydroxyacetophenone and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0088] Comparative Example 3

[0089] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 30wt% of a film stripping agent, 15wt% of an inorganic base, 5wt% of an organic base, 10wt% of a surfactant, 5wt% of an auxiliary agent, and the balance being a solvent.

[0090] The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps:

[0091] S1. In an ice-water bath and under nitrogen protection, 4 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, 25 parts by weight of 1,2-dichloroethane, and 2 parts by weight of trimethylsilyl trifluoromethanesulfonate were mixed, stirred at 35° C. and 600 rpm for 8 hours, and then 40 parts by weight of saturated sodium carbonate aqueous solution were added and stirred for 40 minutes, and the mixture was extracted, separated, washed, and distilled under reduced pressure to obtain intermediate I; 20 parts by weight of 1,2-dichloroethane and 2 parts by weight of 1,6-heptadien-4-ol were added to the obtained intermediate I, and stirred at 35° C. and 600 rpm for 20 minutes, and then 2 parts by weight of saturated sodium carbonate aqueous solution were added. trimethylsilyl trifluoromethanesulfonate, continue stirring for 10 hours, then add 40 parts by weight of saturated sodium carbonate aqueous solution and continue stirring for 40 minutes, extract and separate, wash, and distill under reduced pressure to obtain intermediate II; add 25 parts by weight of dichloromethane and 25 parts by weight of acetonitrile as a mixed solvent to the obtained intermediate II, then add 30 parts by weight of water and 4 parts by weight of sodium periodate, stir at room temperature and 600 rpm for 10 minutes, add 0.1 parts by weight of ruthenium trichloride, stir at 35°C and 600 rpm for 10 hours, add 40 parts by weight of water and stir, adjust the pH to 7.5, extract and separate, wash, and distill under reduced pressure to obtain carboxyl-modified N-acetamidogalactose;

[0092] S2. Mix 1 part by weight of 3-dicarboxyimidopropionic acid, 2 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 30 parts by weight of N,N-dimethylformamide, add 2 parts by weight of the above-mentioned carboxyl-modified N-acetamidogalactose, stir at room temperature and 400 rpm for 4 hours, extract and separate the liquids, wash, and distill under reduced pressure. Dissolve the obtained product in 8 parts by weight of methanol and 1 part by weight of triethylamine, react at 50°C for 24 hours, and remove the solvent by distillation under reduced pressure to obtain a phthalimide derivative.

[0093] The inorganic base is strontium hydroxide.

[0094] The organic base is ethylenediamine.

[0095] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0096] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0097] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0098] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 30 wt% of a stripping agent, 15 wt% of strontium hydroxide, 5 wt% of ethylenediamine, 10 wt% of a surfactant, 5 wt% of 2-fluoro-6-hydroxyacetophenone and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0099] Comparative Example 4

[0100] A film stripping liquid suitable for a flexible circuit board is composed of the following raw materials in percentage by mass: 30wt% of a film stripping agent, 15wt% of an inorganic base, 5wt% of an organic base, 10wt% of a surfactant, 5wt% of an auxiliary agent, and the balance being a solvent.

[0101] The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps:

[0102] Take 1 part by weight of N-hydroxy-4-nitrophthalimide, 2 parts by weight of 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate and 30 parts by weight of N,N-dimethylformamide, mix them, add 2 parts by weight of 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate, stir at room temperature and 400 rpm for 4 hours, extract and separate the liquids, wash, and distill under reduced pressure. The obtained product is dissolved in 8 parts by weight of methanol and 1 part by weight of triethylamine, react at 50°C for 24 hours, and remove the solvent by distillation under reduced pressure to obtain a phthalimide derivative.

[0103] The inorganic base is strontium hydroxide.

[0104] The organic base is ethylenediamine.

[0105] The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyltrimethylammonium bromide in a mass ratio of 1:1.

[0106] The auxiliary agent is 2-fluoro-6-hydroxyacetophenone.

[0107] The solvent is composed of water and diethylene glycol monobutyl ether in a mass ratio of 4:1.

[0108] The method for preparing a stripping liquid suitable for a flexible circuit board comprises the following steps: mixing 30 wt% of a stripping agent, 15 wt% of strontium hydroxide, 5 wt% of ethylenediamine, 10 wt% of a surfactant, 5 wt% of 2-fluoro-6-hydroxyacetophenone and a solvent, and stirring the mixture evenly to obtain a stripping liquid suitable for a flexible circuit board.

[0109] Test Example 1

[0110] Stripping rate test: mSAP process was used and the preparation was carried out in the order of copper substrate-film exposure-development-electroplating copper-washing and drying. The dry film thickness was 25μm and the electroplating copper was 20μm. The test board was then cut into 10cm wide and 8cm test pieces. The line width / dry film width = 20μm / 20μm to obtain a circuit board. The stripping liquid prepared in the above examples 1-3 and comparative examples 1-4 was used to strip the circuit board respectively. The treatment conditions were: the stripping liquid spray pressure was 1.5kg / cm 2 The stripping liquid temperature was 50°C, the stripping time was 3 min, each group was tested 4 times, and the average value was taken. The results are shown in Table 1.

[0111] Table 1 Stripping rate test results

[0112] Stripping rate m / min Stripping residual area Example 1 3.7 No residue Example 2 3.6 No residue Example 3 3.6 No residue Comparative Example 1 2.1 20% Comparative Example 2 3.2 5% Comparative Example 3 3.1 7% Comparative Example 4 2.8 15%

[0113] Test Example 2

[0114] The square resistance test was performed on the circuit board in Test Example 1 before and after treatment to observe the square resistance change rate, square resistance change rate = (square resistance after treatment - square resistance before treatment) / square resistance before treatment * 100%. Four groups were tested in each group and the average value was taken. The results are shown in Table 2.

[0115] Table 2 Square resistance test changes

[0116] Square resistance change rate, % Example 1 0.15% Comparative Example 1 1.2% Comparative Example 2 0.48% Comparative Example 4 0.95%

[0117] From the above results, it can be seen that the stripping solution prepared by the present invention has a good stripping effect on the "dry film" formed in the circuit board, and has little effect on the resistance after treatment. Comparison of Example 1 and Comparative Example 1 shows that the phthalimide derivative prepared by the present invention has a better effect than the direct use of N-hydroxy-4-nitrophthalimide as a stripping agent in Comparative Document 1, because the phthalimide derivative contains nitro, hydroxyl and amide groups, which play different roles in the stripping of the film in the stripping solution: the nitro group enhances the organic solubility of the phthalimide derivative, making it more effective in dissolving the adhesive or adhesive; the presence of the nitro group increases the polarity of the molecule and improves its solubility in organic solvents, thereby promoting the dissolution and stripping of the adhesive. The hydroxyl group increases the surface activity of the phthalimide derivatives, making it easier to form hydrogen bonds or other interactions with the circuit board surface, enhancing the contact between the stripping liquid and the interlayer, which helps to improve the stripping efficiency and speed; the hydroxyl group undergoes a hydrolysis reaction with specific components in the interlayer, destroying the structure of the adhesive and causing the interlayer material to peel off. This hydrolysis can accelerate the separation process of the stripping liquid and the interlayer; it participates in the chemical reaction between the stripping liquid and specific components in the interlayer, accelerating the film peeling process, thereby achieving the interlayer peeling. The amide group gives the phthalimide derivatives the ability to selectively strip specific types of adhesives, which means that they can strip specific components in the circuit board without damaging other materials, thereby ensuring the integrity and quality of the circuit board and reducing the impact on the square resistance of the circuit board.

[0118] By comparing Example 1 and Comparative Example 2, it can be seen that the use of strontium hydroxide in Example 1 is better than directly using sodium hydroxide. The reason is that strontium hydroxide solution is usually milder in alkalinity than sodium hydroxide solution. During use, strontium hydroxide can reduce corrosion and damage to substrates and other materials, reduce the impact on resistance, reduce unnecessary damage or incomplete stripping, and strontium hydroxide can have a better selective stripping effect on specific types of adhesives or resins.

[0119] Further comparison of Example 1 and Comparative Examples 3-4 shows that only the phthalimide derivatives prepared by the specific method of the present invention as the raw material of the stripping solution have a better effect on the "interlayer" treatment of the circuit board. The reason is that the phthalimide derivatives contain nitro, hydroxyl and amide groups, which play different roles in the stripping of the interlayer in the stripping solution. The three groups synergize in the stripping process, each playing its own role, and jointly improve the treatment effect of the "interlayer" in the circuit board, effectively reducing the influence on the square resistance of the circuit board.

Claims

1. A stripping solution suitable for flexible circuit boards, It is characterized in that The method is composed of the following raw materials in percentage by weight: 25-40wt% of a demoulding agent, 10-20wt% of an inorganic base, 3-8wt% of an organic base, 5-12wt% of a surfactant, 3-6wt% of an auxiliary agent, and the balance is a solvent; The demoulding agent is a phthalimide derivative; the preparation method of the phthalimide derivative comprises the following steps: S1, 2-(acetylamino)-2-deoxy-BETA-D-galactose 1,3,4,6-tetraacetate react in 1,2-dichloroethane and trimethylsilyl trifluoromethanesulfonate to obtain intermediate I; 1,6-heptadien-4-ol is added to the obtained intermediate I to react to obtain intermediate II; sodium periodate and water are added to the obtained intermediate II to react in the presence of a catalyst, ruthenium trichloride, to obtain carboxyl-modified N-acetamidogalactose; S2, N-hydroxy-4-nitrophthalimide and the above-mentioned carboxyl-modified N-acetamidogalactose to obtain a phthalimide derivative; The inorganic base is strontium hydroxide; The organic base is ethylenediamine; The surfactant is a mixture of nonylphenol polyoxyethylene ether and octadecyl trimethyl ammonium bromide; The auxiliary agent is 2-fluoro-6-hydroxyacetophenone; The solvent is a mixture of water and diethylene glycol monobutyl ether.

2. The method for preparing a film stripping solution suitable for a flexible circuit board according to claim 1, It is characterized in that The method comprises the following steps: mixing a stripping agent, an inorganic base, an organic base, a surfactant, an auxiliary agent and a solvent, and stirring them evenly to obtain a stripping liquid suitable for a flexible circuit board.