High dielectric metal gate and method for manufacturing the same

During the production process of high dielectric metal gate, multiple step-by-step depositions form a titanium nitride barrier layer and use argon-krillic mixed gas to eliminate suspension phenomenon, the problem of uneven thickness of the barrier layer and wetting layer is solved, and the problem of improvement is improved Filling process and electrical properties of metal gates.

CN118538603BActive Publication Date: 2024-11-12NEXCHIP SEMICON CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410983546.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The existing high-dielectric metal gates have suspension when forming barrier layers and wetting layers, which affects the filling process window and electrical properties of subsequent metal gates.

Method used

The barrier layer of titanium nitride material is formed by performing a step-by-step deposition process multiple times in the gate groove, and the suspension phenomenon is eliminated using a mixture of argon and krypton on the barrier layer to form a uniform wetting layer.

Benefits of technology

It effectively avoids the adhesion of titanium particles and diffusion of metal materials, and improves the regularity and electrical properties of the filling process window of the metal gate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118538603B_ABST
    Figure CN118538603B_ABST
Patent Text Reader

Abstract

The present application discloses a high dielectric metal gate and a method for making the same. The method comprises forming a barrier layer made of titanium nitride material by performing multiple step-by-step deposition processes in a gate groove. The step-by-step deposition process comprises: introducing titanium raw material gas into the gate groove to deposit titanium on the groove wall of the gate groove; introducing nitrogen raw material gas into the gate groove to chemically adsorb the titanium deposited on the groove wall with nitrogen to form one of the titanium nitride films constituting the barrier layer. The present application can improve the process window of subsequent metal gate filling, thereby improving the electrical performance of semiconductor devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a high dielectric metal gate and a method for manufacturing the same. Background Art

[0002] The characteristic size of semiconductor devices continues to decrease according to Moore's Law. When the process node reaches below 28nm, the gate of the semiconductor device adopts a high-K metal gate (HKMG) structure.

[0003] The high dielectric metal gate structure is usually realized by a gate replacement process, that is, a dummy gate structure is first formed in the gate structure formation area, and the dummy gate structure is composed of a gate oxide layer and a polysilicon gate superimposed; then a source region and a drain region are formed on both sides of the dummy gate structure by a source-drain ion implantation process; then the dummy gate structure is removed, and a gate groove is formed in the dummy gate structure removal area; finally, a high dielectric metal gate structure is formed in the gate groove, including forming a gate dielectric layer made of a high dielectric constant dielectric material at the bottom of the gate groove and filling the gate groove to form a functional semiconductor layer and a gate electrode layer made of a metal material, wherein improper filling of the metal material will directly affect the electrical properties of the gate.

[0004] However, some existing functional semiconductor layers including barrier layers and wetting layers will produce obvious overhang phenomenon during the process of depositing titanium nitride (TiN) to form a barrier layer and titanium (Ti) to form a wetting layer using a physical vapor deposition (PVD) process, which is not conducive to the subsequent filling of the metal gate. Summary of the invention

[0005] In view of the above problems, the present application provides a high dielectric metal gate and a method for manufacturing the same, aiming to eliminate the suspension problem of the barrier layer and the wetting layer, improve the process window of the subsequent metal gate filling, and thus improve the electrical performance of the semiconductor device.

[0006] According to a first aspect of the present invention, a method for manufacturing a high dielectric metal gate is provided, comprising forming a barrier layer made of titanium nitride material in a gate groove by performing a step-by-step deposition process multiple times, wherein the step-by-step deposition process comprises:

[0007] Introducing titanium raw material gas into the gate groove to deposit titanium on the groove wall of the gate groove;

[0008] A nitrogen raw material gas is introduced into the gate groove to cause the titanium deposited on the groove wall to chemically adsorb with the nitrogen to form a titanium nitride film which constitutes one of the barrier layers.

[0009] Optionally, the titanium deposited on the groove wall undergoes chemical adsorption with nitrogen to form a titanium nitride film with a thickness of 5-10 angstroms.

[0010] Optionally, the nitrogen raw material gas is nitrogen radicals.

[0011] Optionally, the flow rate of the nitrogen raw gas is 1-20 standard milliliters per minute.

[0012] Optionally, the manufacturing method further comprises forming a wetting layer made of titanium material on the barrier layer in the gate groove, and the formation process of the wetting layer comprises:

[0013] Introducing titanium raw material gas into the gate groove to deposit titanium on the barrier layer;

[0014] A mixed gas of argon and krypton is passed into the gate groove so that the mixed gas bombards the titanium deposited on the barrier layer at the notch of the gate groove.

[0015] Optionally, the flow rate of argon gas in the mixed gas is 50-1000 standard milliliters per minute, and the flow rate of krypton gas is 1-200 standard milliliters per minute.

[0016] Optionally, after the mixed gas bombards the titanium deposited on the barrier layer at the notch of the gate groove, the manufacturing method further includes: introducing titanium raw material gas into the gate groove to deposit titanium on the wetting layer to form a repair film for the wetting layer.

[0017] Optionally, the repair film has a thickness of 20-50 angstroms.

[0018] Optionally, titanium is deposited on the groove wall of the gate groove and on the barrier layer by introducing titanium raw material gas into the gate groove through a physical vapor deposition process, and the DC power of the physical vapor deposition process is 10-50 kilowatts.

[0019] According to a second aspect of the present invention, a high dielectric metal gate is provided. The high dielectric metal gate is manufactured by any one of the manufacturing methods described in the first aspect.

[0020] The unexpected technical effects of this application are:

[0021] According to the method for manufacturing a high dielectric metal gate provided in an embodiment of the present application, a barrier layer made of titanium nitride material is formed by performing a step-by-step deposition process in a gate groove multiple times, and the step-by-step deposition process includes: introducing titanium raw material gas into the gate groove to deposit titanium on the groove wall of the gate groove; and introducing nitrogen raw material gas into the gate groove to chemically adsorb the titanium deposited on the groove wall with nitrogen to form one of the titanium nitride films constituting the barrier layer. In this process, since the barrier layer is formed by performing a step-by-step deposition process for many times, the titanium deposited in the previous step of each step-by-step deposition process is relatively thin, so that the deposited titanium can fully contact the nitrogen raw material gas introduced in the next step, not only the titanium deposited at the gate groove can be fully treated by the nitrogen raw material gas to reduce the surface energy, but also the titanium deposited on the entire groove wall of the gate groove can fully react with nitrogen to obtain titanium nitride. Among them, the former achieves the effect of reducing the adhesion of titanium particles, thereby effectively avoiding the occurrence of the hanging phenomenon; the latter achieves the effect of making the formed titanium nitride more uniform, thereby effectively preventing the diffusion of metal materials in the gate electrode layer to the work function layer on the other side of the barrier layer, which is of great significance to improving the electrical properties of the gate.

[0022] Furthermore, the method for manufacturing a high dielectric metal gate according to the embodiment of the present application also includes forming a wetting layer made of titanium material on the barrier layer of the gate groove, and the formation process of the wetting layer includes: introducing titanium raw material gas into the gate groove to deposit titanium on the barrier layer; and passing a mixed gas of argon and krypton into the gate groove to bombard the titanium deposited on the barrier layer at the notch of the gate groove. Since argon is easy to ignite and krypton has a large atomic number and a large mass advantage, the mixed gas obtained by combining argon and krypton can effectively bombard the titanium deposited on the barrier layer at the notch of the gate groove, thereby eliminating the phenomenon of titanium hanging. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The above and other objects, features and advantages of the present application will become more apparent through the following description of the embodiments of the present application with reference to the accompanying drawings, in which:

[0024] Figure 1 A cross-sectional view of a semiconductor device is shown;

[0025] Figure 2 A partial structural cross-sectional view of a high dielectric metal gate made by prior art is shown;

[0026] Figure 3a A cross-sectional view of a substrate for forming a barrier layer according to an embodiment of the present application is shown;

[0027] Figure 3b According to the embodiment of the present application, Figure 3a A schematic diagram of forming a barrier layer on the substrate shown;

[0028] Figure 3c According to the embodiment of the present application, Figure 3b Schematic diagram of forming a wetting layer on the barrier layer shown;

[0029] Figure 3d According to the embodiment of the present application, Figure 3c Schematic diagram of filling the gate electrode layer in the cavity formed by the wetting layer;

[0030] Figure 4 A flowchart showing an exemplary method of forming a barrier layer by performing a step-by-step deposition process multiple times according to an embodiment of the present application is shown;

[0031] Figure 5a A cross-sectional view showing a substrate for depositing titanium according to an embodiment of the present application;

[0032] Figure 5b According to the embodiment of the present application, Figure 5a Schematic diagram of titanium deposition on the substrate shown;

[0033] Figure 5c The embodiment according to the present application is shown Figure 5b Schematic diagram of the deposited titanium forming a titanium nitride film;

[0034] Figure 5d According to the embodiment of the present application, Figure 5c Schematic diagram of titanium deposited on the formed titanium nitride film shown;

[0035] Figure 5e The embodiment according to the present application is shown Figure 5d Schematic diagram of the deposited titanium forming a titanium nitride film;

[0036] Figure 6 A flow chart showing the formation of a wetting layer according to an embodiment of the present application;

[0037] Figure 7a A schematic diagram showing the deposition of titanium on a barrier layer according to an embodiment of the present application;

[0038] Figure 7b The embodiment of the present application is shown Figure 7a Schematic diagram of bombardment of deposited titanium shown;

[0039] Figure 7c The embodiment according to the present application is shown Figure 7b Schematic diagram showing the results of the bombardment process. DETAILED DESCRIPTION

[0040] The present application will be described in more detail below with reference to the accompanying drawings. In each of the accompanying drawings, the same elements are represented by similar reference numerals. For the sake of clarity, the various parts in the accompanying drawings are not drawn to scale. In addition, some well-known parts may not be shown.

[0041] This application may be presented in a variety of forms, some examples of which are described below.

[0042] In the rapid development of semiconductor manufacturing technology, MOS (Metal Oxide Semiconductor) devices are shrinking, and the thickness of the gate oxide layer in MOS devices is decreasing. Too small a gate oxide layer thickness will cause a significant carrier tunneling effect, and a high-dielectric metal gate structure is used to solve this problem.

[0043] In the high-k metal gate structure, high-k dielectric materials replace conventional materials such as silicon oxide as the gate dielectric layer of the MOS device, thereby avoiding the occurrence of carrier tunneling effect caused by the reduction of the thickness of the gate dielectric layer. At the same time, due to the pinning effect of the Fermi level between the high-k dielectric material and the semiconductor substrate, it is necessary to use metal materials to replace conventional materials such as polysilicon as the gate electrode layer of the MOS device. The change of the gate electrode layer material affects the work function difference between the gate and the substrate, so it is also necessary to set a work function layer between the gate dielectric layer and the gate electrode layer to adjust the threshold voltage of the gate to an appropriate value.

[0044] Figure 1 A schematic cross-sectional view of a semiconductor device is shown. The semiconductor device 100 is, for example, a MOSFET (Metal Oxide Semiconductor Field Effect Transistor), but is not limited thereto.

[0045] like Figure 1As shown, the semiconductor device 100 includes a substrate 101. For an N-type MOSFET, the substrate 101 is doped with a P-type, and for a P-type MOSFET, the substrate 101 is doped with an N-type. The semiconductor device 100 also includes a source region 102 and a drain region 103 located in the substrate 101. The source region 102 and the drain region 103 are formed by implanting ions into the substrate 101. For an N-type MOSFET, the source region 103 and the drain region 104 are doped with an N-type, and for a P-type MOSFET, the source region 103 and the drain region 104 are doped with a P-type. Between the source region 102 and the drain region 103 is a channel of the semiconductor device 100. The semiconductor device 100 also includes an interlayer dielectric layer 104 located on the substrate 101 and a gate groove located on the channel in the interlayer dielectric layer 104, and the bottom of the gate groove contacts the surface of the substrate 101. The high-K metal gate structure is usually realized by a gate replacement process, and thus a pseudo gate structure consisting of a gate oxide layer and a polysilicon gate is first formed in the formation area of ​​the gate structure in the interlayer dielectric layer 104, and then a source region 102 and a drain region 103 are formed in the substrate 101 on both sides of the pseudo gate structure by a source-drain ion implantation process, and then the pseudo gate structure is removed to form the gate groove mentioned above and the final high-K metal gate structure is formed by filling the gate groove.

[0046] like Figure 1 As shown, the filling of the gate groove includes forming a gate dielectric layer 105 made of a high dielectric constant dielectric material at the bottom of the gate groove, and filling the gate groove to form a functional semiconductor layer 106 and a gate electrode layer 107 made of a metal material. Specifically, the functional semiconductor layer 106 covers the gate dielectric layer 105 at the bottom of the groove and the interlayer dielectric layer 104 on the sidewall of the groove, and the gate electrode layer 107 is formed in the cavity formed by the functional semiconductor layer 106. The high dielectric constant dielectric material for making the gate dielectric layer 105 is, for example, hafnium dioxide, and the metal material for making the gate electrode layer 107 is, for example, aluminum.

[0047] Figure 2 FIG. 1 is a partial structural schematic diagram of a high dielectric metal gate structure formed in a gate groove using the prior art. Figure 2 , the functional semiconductor layer 106 includes a work function layer 1061, a barrier layer 1062 and a wetting layer 1063. Specifically, the wetting layer 1063 is used to wet the barrier layer 1062 so that the metal material for the subsequent production of the gate electrode layer 107 can flow more smoothly from the notch of the gate groove to the cavity formed by the functional semiconductor layer 106, so the wetting layer 1063 is on the surface of the functional semiconductor layer 106 adjacent to the gate electrode layer 107, and the wetting layer 1063 exists in the gate groove in a manner of covering the barrier layer 1062; the barrier layer 1062 is used to prevent the metal material in the gate electrode layer 107 from diffusing to the work function layer 1061, so the barrier layer 1062 exists in the gate groove in a manner of covering the work function layer 1061.

[0048] It should be noted that the functional semiconductor layer 106 includes but is not limited to the functional structural layers shown above. For example, in some examples, the functional semiconductor layer 106 may also include an etching stop layer covered by the work function layer 1061 .

[0049] The work function layer 1061 adopts different structures or different materials due to different types of semiconductor devices 100. For example, for a P-type MOSFET, the work function layer 1061 includes a first work function layer and a second work function layer, the second work function layer is located between the first work function layer and the barrier layer 1062, the first work function layer adopts titanium nitride, and the second work function layer adopts titanium aluminum alloy; for an N-type MOSFET, the work function layer 1061 only includes a layer made of titanium aluminum alloy. The barrier layer 1062 adopts titanium nitride, and the wetting layer 1063 adopts titanium.

[0050] At present, below the 28nm process node, a physical vapor deposition process is used to deposit titanium nitride to form the barrier layer 1062 and titanium to form the wetting layer 1063. However, this process will produce an obvious hanging phenomenon, such as Figure 2 As shown, the thickness of the barrier layer 1062 and the wetting layer 1063 are respectively uneven, and each has a larger thickness at the corner of the gate groove notch, so that the process window for metal material filling when the subsequent gate electrode layer 107 is formed is reduced and irregular, which is not conducive to the subsequent filling of the metal material, and further the poor filling of the metal material causes the gate electrical properties to be adversely affected.

[0051] In view of this, an embodiment of the present application provides a method for manufacturing a high dielectric metal gate. The method improves the barrier layer forming process so that Figure 3a The substrate 201 shown is Figure 3b The barrier layer 202 is formed as shown, and the thickness of the barrier layer 202 is uniform and there is no hanging phenomenon. The substrate 201 is a general term for the work function layer included in the functional semiconductor layer in the high dielectric metal gate structure and various functional structural layers covered by the work function layer. Further, the manufacturing method improves the wetting layer formation process, so that Figure 3b The barrier layer 202 shown is as shown in FIG. Figure 3c As shown in the figure, a wetting layer 203 is formed, and the thickness of the formed wetting layer 203 is uniform, and there is no hanging phenomenon. Therefore, the process window of the subsequent metal gate filling is relatively regular, and there is no problem of the gate groove notch shrinking. Figure 3c The cavities formed by the wetting layer 203 are filled with metal materials, such as Figure 3d As shown in FIG. 1 , a gate electrode layer 204 with good electrical properties is formed, thereby completing a partial structure such as Figure 3d The manufacturing process of the high dielectric metal gate 200 is shown.

[0052] The method for manufacturing a high dielectric metal gate provided in an embodiment of the present application includes forming a barrier layer 202 made of titanium nitride material by performing a step-by-step deposition process multiple times in a gate groove, that is, each step-by-step deposition process forms one layer of the titanium nitride film constituting the barrier layer 202, and the multiple layers of titanium nitride films formed by performing the step-by-step deposition process multiple times are stacked to form the barrier layer 202. Figure 4 FIG. 2 is a schematic diagram of an exemplary process of forming the barrier layer 202 by performing a step-by-step deposition process multiple times. The step-by-step deposition process is performed once and includes: Figure 4 The steps S110 and S120 are each performed once. Figure 4 As shown, the process of forming the barrier layer 202 may include:

[0053] Step S110, introducing titanium raw material gas into the gate groove to deposit titanium on the groove wall of the gate groove;

[0054] In step S120 , nitrogen source gas is introduced into the gate groove to cause the titanium deposited on the groove wall to chemically adsorb with nitrogen to form a titanium nitride film that constitutes one of the barrier layers 202 .

[0055] In step S103, it is determined whether the number of executions of the step-by-step deposition process is the preset number. If the number of executions of the step-by-step deposition process is not the preset number, the process returns to step S110. If the number of executions of the step-by-step deposition process is the preset number, the process of forming the barrier layer 202 is terminated.

[0056] It should be understood that when the first step-by-step deposition process is performed, step S110 is to deposit titanium on the substrate 201 in the gate groove, and when the subsequent step-by-step deposition process is performed, step S110 is to deposit titanium on the titanium nitride film formed in the previous step. The formation process of the above-mentioned barrier layer 202 is an alternating cycle execution process of step S110 and step S120.

[0057] In one example, the method for manufacturing a high dielectric metal gate provided in an embodiment of the present application forms a barrier layer 202 made of titanium nitride material in the gate groove by performing a step-by-step deposition process twice, that is, the preset number of times described in the above step S130 is twice. Specifically, step S110 is performed once. Figure 5a The substrate 201 shown is Figure 5b As shown in the figure, titanium is deposited, and then step S120 is performed once to make Figure 5b The titanium deposited as shown Figure 5c As shown in FIG. 1 , the titanium nitride film is chemically adsorbed by contacting nitrogen, thus completing a step-by-step deposition process to form one of the titanium nitride films constituting the barrier layer 202; then step S110 is performed again to form a titanium nitride film on the titanium nitride film formed in the previous distributed deposition process. Figure 5dTitanium is deposited as shown, and then step S120 is performed again to make Figure 5d The titanium deposited as shown Figure 5e As shown, the titanium nitride film is chemically adsorbed by contact with nitrogen, thus completing another step-by-step deposition process to form another titanium nitride film constituting the barrier layer 202. The barrier layer 202 is formed by stacking two titanium nitride films.

[0058] The titanium raw material gas includes a large number of titanium particles, and the titanium particles can be titanium atoms sputtered in the physical vapor deposition process; the nitrogen raw material gas includes a large number of nitrogen particles, and the nitrogen particles can be nitrogen free radicals, so that in the chemical adsorption process of titanium and nitrogen described in step S120, titanium and nitrogen can quickly react chemically to generate titanium nitride. Nitrogen free radicals can be generated by a radio frequency plasma source with a power of 10-2000W. The chemical adsorption process of titanium and nitrogen can be carried out at room temperature. It should be noted that in the chemical adsorption process of titanium and nitrogen, on the one hand, titanium and nitrogen will react chemically to generate titanium nitride; on the other hand, the newly deposited titanium must undergo nitrogen passivation treatment, that is, the nitrogen raw material gas also plays a role in reducing the surface energy of the newly deposited titanium.

[0059] When nitrogen raw material gas is introduced into the gate groove in step S120, the flow rate of nitrogen raw material gas should not be too small or too large. If the flow rate of nitrogen raw material gas is too small, part of the titanium deposited in step S110 will inevitably need a long time to fully contact the nitrogen particles. The titanium particles that are not fully contacted with the nitrogen particles during this period will be adsorbed together due to the effect of surface energy, especially the adsorption of titanium particles at the notch of the gate groove will still cause a certain degree of suspension phenomenon; on the contrary, if the flow rate of nitrogen raw material gas is too large, it will easily lead to poor stability of process pressure, affect the uniformity and stability of the formed titanium nitride film, and also cause unnecessary waste of process resources and costs. For this reason, in the embodiment of the present application, the flow rate of nitrogen raw material gas is set to 1-20 standard milliliters / minute.

[0060] The barrier layer 202 made of titanium nitride material is formed by performing a step-by-step deposition process multiple times in the gate groove. Therefore, the titanium nitride film formed by each step-by-step deposition process is allowed to be thinner, but the titanium nitride film should not be too thin or too thick. If the titanium nitride film is too thick, the titanium to be deposited once in step S110 will be thicker, which is not conducive to the subsequent full contact between the nitrogen raw material gas and the titanium particles; conversely, if the titanium nitride film is too thin, in order to achieve the thickness of the barrier layer 202, it is necessary to perform the step-by-step deposition process multiple times, which affects the process efficiency. For this reason, in the embodiment of the present application, the titanium nitride film formed by each step-by-step deposition process is set to a thickness of 5-10 angstroms.

[0061] In the above-mentioned process of forming the barrier layer 202, since the barrier layer 202 is formed by performing a step-by-step deposition process for many times, the titanium deposited in step S110 in each step-by-step deposition process is relatively thin, so that the deposited titanium can fully contact the nitrogen raw material gas introduced in step S120, which not only allows the titanium deposited at the gate groove to be fully treated by the nitrogen raw material gas to reduce the surface energy, but also allows the titanium deposited on the entire groove wall of the gate groove to fully react with nitrogen to obtain titanium nitride. Among them, the former achieves the effect of reducing the adhesion of titanium particles, thereby effectively avoiding the occurrence of the hanging phenomenon; the latter achieves the effect of making the formed titanium nitride more uniform, thereby effectively preventing the diffusion of metal materials in the gate electrode layer to the work function layer on the other side of the barrier layer, which is of great significance to improving the gate electrical properties.

[0062] Figure 6 FIG. 2 is a flow chart of forming a wetting layer 203 made of titanium material on a barrier layer 202 in a method for manufacturing a high dielectric metal gate provided in an embodiment of the present application. Figure 6 As shown, the formation process of the wetting layer 203 includes:

[0063] Step S140, introducing titanium raw material gas into the gate groove to deposit titanium on the barrier layer 202;

[0064] In step S150 , a mixed gas of argon and krypton is introduced into the gate groove to allow the mixed gas to bombard the titanium deposited on the barrier layer 202 at the notch of the gate groove.

[0065] It should be understood that the wetting layer 203 is formed by executing step S140 and step S150 once each, so the thickness of the titanium deposited in step S140 is determined according to the required thickness of the wetting layer 203, and the execution of step S150 is used to bombard a portion of the titanium deposited on the barrier layer 202 at the notch of the gate groove, thereby removing the hanging phenomenon.

[0066] Figure 7a FIG. 2 is a schematic diagram showing the deposition of titanium on the barrier layer 202. Since the titanium raw material gas introduced in step S140 will pass through the gate groove notch, more titanium particles will be deposited at the gate groove notch due to the surface energy of the titanium particles. When the titanium deposited on the barrier layer 202 reaches the required thickness of the wetting layer 203, the gate groove notch will appear as shown in FIG. Figure 7a The hanging phenomenon shown. Figure 7b The following is shown in step S150. Figure 7a Schematic diagram of bombardment of deposited titanium shown in FIG. Due to the occurrence of the suspension phenomenon, more particles in the mixed gas bombard the gate groove notch, so that the titanium particles deposited at the gate groove notch are formed after sufficient bombardment. Figure 7c The result shown is that the hanging phenomenon is eliminated.

[0067] Furthermore, in the process of bombarding the titanium deposited on the barrier layer 202 at the notch of the gate groove by the mixed gas in step S150, other parts will also be bombarded unnecessarily, so that the titanium deposited on the barrier layer 202 is thinned as a whole, and thus titanium raw material gas can be introduced into the gate groove after step S150 to deposit titanium on the wetting layer 203 to form a repair film of the wetting layer 203. The thickness of the repair film can be selected to be 20-50 angstroms, so as to achieve the effect of repairing the wetting layer 203 in thickness.

[0068] The reason why the mixed gas of argon and krypton is used for bombardment is that both argon and krypton are inert elements. Therefore, when the mixed gas bombards the titanium deposited on the barrier layer 202, the titanium will not react chemically due to contact with the titanium, so that the quality of the wetting layer 203 will not be affected. In addition, argon is easy to ignite, so argon atoms are easily ionized into argon ions and electrons, and the mixed krypton atoms are easily ionized into krypton ions and electrons by the impact of particles ionized by argon atoms. Krypton has a large atomic number (the atomic number of argon is 18 and the atomic number of krypton is 36) and has a large mass advantage. Therefore, under the action of the electric field, the argon ions and krypton ions can effectively bombard the titanium deposited on the barrier layer 202 at the notch of the gate groove, thereby eliminating the phenomenon of titanium hanging.

[0069] The flow rates of argon and krypton in the above-mentioned mixed gas should not be too small or too large. If the flow rate of argon or krypton is too small, the impact force of the mixed gas on the titanium deposited on the barrier layer 202 at the notch of the gate groove is insufficient; on the contrary, if the flow rate of argon or krypton is too large, the impact force of the mixed gas on the titanium deposited on the barrier layer 202 at the notch of the gate groove is too large, and the titanium particles impacted will also have a greater impact force on the titanium deposited on the barrier layer 202 in the surrounding area. In addition, more mixed gas will enter the gate groove and strongly impact the titanium deposited on the inner side wall and the bottom of the barrier layer 202 of the gate groove. In this way, most areas of the titanium deposited on the barrier layer 202 will be hit with greater force, so that the wetting layer 203 formed by the deposition of titanium is more seriously damaged. In addition, the ratio of the flow rate of argon gas to the flow rate of krypton gas in the mixed gas should not be too small or too large. If the ratio of the argon flow rate to the krypton flow rate in the mixed gas is too small, there is too little argon in the mixed gas, so that the particles ionized by the argon are not enough to ionize all the krypton atoms in the mixed gas; on the contrary, if the ratio of the argon flow rate to the krypton flow rate in the mixed gas is too large, there is too much argon in the mixed gas, so that although the ions ionized by the argon are enough to ionize the krypton atoms in the mixed gas, the argon does not contribute much to the impact force, so there is a problem of argon waste. For this reason, in the embodiment of the present application, the flow rate of argon in the above-mentioned mixed gas is set to 50-1000 standard milliliters per minute, and the flow rate of krypton is set to 1-200 standard milliliters per minute.

[0070] The deposition of titanium on the groove wall of the gate groove in the above step S110 and the deposition of titanium on the barrier layer 202 in the step S140 are carried out by introducing titanium raw material gas into the gate groove through a physical vapor deposition process. The DC power of the physical vapor deposition process should not be too small or too large. If the DC power of the physical vapor deposition process is too large, it is easy to cause the titanium deposited on the groove wall of the gate groove and the barrier layer 202 to be too thick, and it is difficult to meet the thickness requirements of the barrier layer 202 and the wetting layer 203; on the contrary, if the DC power of the physical vapor deposition process is too small, it is not only easy to cause the titanium deposited on the groove wall of the gate groove and the barrier layer 202 to be too thin, but also easy to reduce the deposition rate and deposition stability of titanium. For this reason, in the embodiment of the present application, the DC power of the above physical vapor deposition process is set to 10-50 kilowatts.

[0071] Corresponding to the manufacturing method of the high dielectric metal gate provided in the above embodiments, another embodiment of the present application further provides a high dielectric metal gate, which is manufactured by any of the manufacturing methods provided in the above embodiments and has excellent electrical properties. Figure 3d The structure shown is an exemplary structure of a portion of the high dielectric metal gate structure provided in the embodiment of the present application. It should be understood that Figure 3d The structures of the barrier layer 202 and the wetting layer 203 are mainly shown, so as to illustrate that the gate electrode layer 204 has a regular and non-shrinking process window when being filled. Figure 3d The structure shown does not limit all structures of the high dielectric metal gate provided in the embodiments of the present application.

[0072] The embodiments of the present application are described above, and these embodiments do not describe all the details in detail, nor do they limit the application to the specific embodiments described. Obviously, many modifications and changes can be made based on the above description. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present application, so that those skilled in the art can make good use of the present application and the modifications based on the present application. The present application is only limited by the claims and their full scope and equivalents.

Claims

1. A method for manufacturing a high dielectric metal gate, comprising forming a barrier layer made of titanium nitride material in a gate groove by performing a step-by-step deposition process multiple times and forming a wetting layer made of titanium material on the barrier layer in the gate groove, wherein: The step-by-step deposition process includes: introducing titanium raw material gas into the gate groove to deposit titanium on the groove wall of the gate groove; introducing nitrogen raw material gas into the gate groove to chemically adsorb the titanium deposited on the groove wall with nitrogen to form one of the titanium nitride films constituting the barrier layer; The formation process of the wetting layer includes: introducing titanium raw material gas into the gate groove to deposit titanium on the barrier layer; and introducing a mixed gas of argon and krypton into the gate groove to bombard the titanium deposited on the barrier layer at the notch of the gate groove.

2. The method according to claim 1, wherein: The titanium deposited on the groove wall undergoes chemical adsorption with nitrogen to form a titanium nitride film with a thickness of 5-10 angstroms.

3. The method according to claim 1, wherein: The nitrogen raw material gas is nitrogen radicals.

4. The method according to claim 1, wherein: The flow rate of the nitrogen raw gas is 1-20 standard milliliters per minute.

5. The method according to claim 1, wherein: The flow rate of argon gas in the mixed gas is 50-1000 standard milliliters per minute, and the flow rate of krypton gas is 1-200 standard milliliters per minute.

6. The manufacturing method according to claim 1, after the mixed gas bombards the titanium deposited on the barrier layer at the notch of the gate groove, further comprising: A titanium raw material gas is introduced into the gate groove to deposit titanium on the wetting layer to form a repair film for the wetting layer.

7. The method according to claim 6, wherein: The thickness of the repair film is 20-50 angstroms.

8. The method according to claim 1, wherein: Titanium is deposited on the groove wall of the gate groove and on the barrier layer by introducing titanium raw material gas into the gate groove through a physical vapor deposition process, and the direct current power of the physical vapor deposition process is 10-50 kilowatts.

9. A high dielectric metal gate, wherein the high dielectric metal gate is manufactured by the manufacturing method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor devices

    CN102956455A

  • Semiconductor device manufacturing method

    CN103137489A

  • Titanium nitride film preparation method and device

    CN113388825A

  • Semiconductor gate structure and preparation method thereof

    CN114744030A

  • Semiconductor device and manufacturing method thereof

    CN115497919A