Cement grinding enhancement powder and preparation method thereof
By coating nano-silica with polydopamine and treating it with other compounds, cement grinding-aid reinforcement powder is prepared, which solves the problem of high energy consumption and waste of resources in cement grinding, improves the dispersion and strength of cement, prevents electrostatic aggregation, and prolongs the The grinding limit improves the overall performance of cement.
Patent Information
- Application Number
- CN202411024257.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-29
AI Technical Summary
During the cement grinding process, energy consumption is high and energy utilization is low. The poor wear resistance of clinker and mixed materials leads to a waste of resources. Static electricity and water vapor in the mill cause balling and forging phenomena, which affects cement output and quality.
Polydopamine is used to coat nano-silica, and it is hyperbranched with silane coupling agent, acrylic acid, isopentenyl polyoxyethylene ether, maleic anhydride, etc., and combined with sodium chloride and sodium tripolyphosphate to prepare cement additives. Grind reinforced powder and improve dispersion and strength through ball milling.
Reduce the energy consumption of cement powder, improve the dispersion and strength of cement, prevent electrostatic agglomeration, reduce ball wrapping, extend the grinding limit, and improve the overall performance of cement.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement, and in particular to a cement grinding aid and enhancement powder and a preparation method thereof. Background Art
[0002] Cement is one of the basic materials in the construction industry and is widely used in the fields of road, bridge, and house construction. The production and sales volume of cement in my country is huge, but the cement industry is a heavy industry and a high-energy-consuming industry, mainly because the cement production process requires the grinding of cement raw materials and clinkers, and the energy consumption in the grinding process is high and the energy utilization rate is extremely low. Because when the cement particles are refined, they tend to agglomerate automatically due to their large surface energy. Cement grinding includes two methods: separate grinding and mixed grinding. The more commonly used method is mixed grinding. During mixed grinding, due to the difference in wear resistance between the clinker and the admixture in cement, the performance of the clinker cannot be fully utilized, resulting in a waste of resources. Moreover, when the clinker and admixtures in cement are added to the mill for grinding together, the materials will generate static electricity due to the intense and frequent friction and impact between the materials and between the materials and the grinding bodies. These charged materials will be adsorbed on the surface of the steel balls and the grinding bodies, causing serious ball and forging phenomena in the cement mill. When the humidity of the added admixture is higher than 5%, a large amount of water vapor will be generated in the mill, increasing the humidity of the grinding materials, which will also cause the above-mentioned ball and forging phenomena, greatly reducing the cement production and quality.
[0003] At present, cement grinding aids commonly used at home and abroad are mainly composed of alcohol amine substances such as triethanolamine and its composite product, which have good use effect. Most of these grinding aids are small molecule composite grinding aids, which have remarkable effects, but poor performance stability and are sensitive to the change of dosage. Another cement grinding aid that is widely studied now is a polymer synthetic grinding aid, which combines various functional groups into a molecular chain structure, has obvious grinding aid enhancement effect, and its dosage has little effect on cement performance, and better ensures that production safety is carried out. However, there are often some high costs, some are complicated preparation processes, some have unsatisfactory effects, some have poor compatibility with concrete admixtures, etc. Summary of the invention
[0004] The purpose of the present invention is to provide a cement grinding-aiding and reinforcing powder and a preparation method thereof, which can reduce energy consumption, have a grinding-aiding effect on cement powder, improve the dispersibility of cement, have a certain early strength effect on the output cement, improve the strength of cement, and at the same time, promote the hydration of cement minerals and improve the comprehensive performance of cement.
[0005] The technical solution of the present invention is achieved in this way:
[0006] The invention provides a method for preparing cement grinding aid and reinforcing powder. The method comprises the following steps: coating nano silicon dioxide with polydopamine, modifying the surface with a silane coupling agent, reacting with dimethylol propionic acid under the catalysis of p-toluenesulfonic acid to obtain hyperbranched nanoparticles, copolymerizing with acrylic acid, isopentenyl polyoxyethylene ether and maleic anhydride, filtering, washing, drying, mixing with sodium chloride and sodium tripolyphosphate, ball milling and drying to obtain cement grinding aid and reinforcing powder.
[0007] As a further improvement of the present invention, the following steps are included:
[0008] S1. Polydopamine coating: adding nano-silica to water, adding dopamine hydrochloride and a catalyst, heating and stirring to react, centrifuging, washing, and drying to obtain polydopamine-modified nano-silica;
[0009] S2. Preparation of modified nano-silica: The polydopamine-modified nano-silica obtained in step S1 was added to ethanol, a silane coupling agent was added, the reaction was heated and stirred, centrifuged, washed, and dried to obtain modified nano-silica;
[0010] S3 preparation of hyperbranched nanoparticles: the modified nano-silica prepared in step S2 was added to xylene, dimethylol propionic acid, p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0011] S4. Preparation of inorganic salt: sodium chloride and sodium tripolyphosphate were mixed to obtain an inorganic salt;
[0012] S5. Preparation of cement grinding aid enhancing powder: acrylic acid, isopentenyl polyoxyethylene ether, maleic anhydride and the hyperbranched nanoparticles obtained in step S3 are added to water, and under the protection of inert gas, an initiator system is added, and the reaction is heated and stirred. The product is filtered, washed, and dried, and mixed with the inorganic salt obtained in step S4, ball-milled, and dried to obtain cement grinding aid enhancing powder.
[0013] As a further improvement of the present invention, the mass ratio of the nano-silicon dioxide, dopamine hydrochloride and catalyst in step S1 is 10: (12-15): (1-2), the catalyst is a Tris-HCl solution with a pH of 8.5-9.5, the average particle size of the nano-silicon dioxide is 80-120 nm, the temperature of the heating and stirring reaction is 45-55° C., and the time is 2-4 h.
[0014] As a further improvement of the present invention, the mass ratio of the polydopamine-modified nano-silica to the silane coupling agent in step S2 is 10:(2-3), the silane coupling agent is a silane coupling agent with a double bond, selected from at least one of KH570, A151, and A171, and the temperature of the heating and stirring reaction is 40-50° C., and the time is 1-3 h.
[0015] As a further improvement of the present invention, the mass ratio of the modified nano-silica, dimethylolpropionic acid and p-toluenesulfonic acid in step S3 is (10-15): (7-10): (0.07-0.1), and the stirring reaction time is 5-7h.
[0016] As a further improvement of the present invention, the mass ratio of sodium chloride to sodium tripolyphosphate in step S4 is (1-2):10.
[0017] As a further improvement of the present invention, the mass ratio of acrylic acid, isopentenyl polyoxyethylene ether, maleic anhydride, hyperbranched nanoparticles, and inorganic salt in step S5 is (5-7): (2-3): (1-2): (8-12): (1-2), the initiator system includes an initiator and sodium sulfite in a mass ratio of (3-5): 2, the initiator is selected from at least one of potassium persulfate, sodium persulfate, and ammonium persulfate, the temperature of the heating and stirring reaction is 55-65° C., the time is 3-5 hours, and the ball milling time is 1-3 hours.
[0018] As a further improvement of the present invention, the present invention specifically comprises the following steps:
[0019] S1. Polydopamine coating: 10 parts by weight of nano-silica was added to water, 12-15 parts by weight of dopamine hydrochloride and 1-2 parts by weight of a catalyst were added, heated to 45-55°C, stirred for 2-4h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0020] The catalyst is a Tris-HCl solution with a pH of 8.5-9.5;
[0021] S2. Preparation of modified nano-silica: 10 parts by weight of the polydopamine-modified nano-silica prepared in step S1 was added to ethanol, 2-3 parts by weight of a silane coupling agent was added, heated to 40-50 ° C, stirred for 1-3h, centrifuged, washed, and dried to obtain modified nano-silica;
[0022] S3 preparation of hyperbranched nanoparticles: 10-15 parts by weight of the modified nano-silica obtained in step S2 was added to xylene, 7-10 parts by weight of dimethylol propionic acid, 0.07-0.1 parts by weight of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 5-7h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0023] S4 Preparation of an inorganic salt: 1-2 parts by weight of sodium chloride, 10 parts by weight of sodium tripolyphosphate were stirred and mixed to obtain an inorganic salt;
[0024] S5. Preparation of cement grinding aid enhancing powder: 5-7 parts by weight of acrylic acid, 2-3 parts by weight of isopentyl polyoxyethylene ether, 1-2 parts by weight of maleic anhydride and 8-12 parts by weight of the hyperbranched nanoparticles obtained in step S3 are added to water, under inert gas protection, 0.01-0.02 parts by weight of the initiator system is added, heated to 55-65 ° C, stirred for 3-5h, the product is filtered, washed, dried, and mixed with 1-2 parts by weight of the inorganic salt obtained in step S4 and ball milled for 1-3h, dried to obtain cement grinding aid enhancing powder;
[0025] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 3-5:2.
[0026] The present invention further protects a cement grinding aid and enhancement powder prepared by the above preparation method.
[0027] The present invention has the following beneficial effects:
[0028] The present invention uses nano-silicon dioxide as the core. The nano-particles can form new crystals with the mineral particles and cementitious materials in the cement-based materials, thereby improving the strength and hardness of the cement-based materials. At the same time, the nano-particles can form a protective film to prevent moisture and harmful substances from penetrating into the material, thereby extending the life of the material.
[0029] By coating modified nano-silica with polydopamine, it has abundant amino groups on its surface, which can subsequently undergo hyperbranching reaction with dimethylol propionic acid to form a hyperbranching modifier. After being modified with a silane coupling agent with double bonds, the surface of the nanoparticles has double bonds, which can undergo polymerization reaction with monomers such as acrylic acid, isopentyl polyoxyethylene ether, and maleic anhydride to connect to the polymer chain, thereby improving the dispersibility and compatibility of the nanomaterials and effectively avoiding the problems of agglomeration of nanoparticles. The polymer obtained by polymerization achieves the dispersion and hydration induction of cement particles by relying on its surface active dispersing properties and the repulsive effect of the functional groups;
[0030] Sodium chloride has a grinding aid effect on cement powder, and sodium tripolyphosphate has a retarding effect on cement. Under the combined effect, the grinding aid effect on cement is obvious, the strength of cement is significantly improved, and there is a synergistic effect.
[0031] The cement grinding enhancement powder of the present invention is adsorbed on the surface of the particles of the grinding material to reduce the friction and adhesion between the particles, make the sliding between the particles easier, increase the fluidity of the material, improve the grinding environment in the mill, improve the grinding effect, and can also effectively prevent or reduce the agglomeration phenomenon, balance the static electricity on the surface of the particles, reduce the surface tension and surface energy, shield the electrostatic cohesion between the particles, eliminate the ball-wrapping and paste grinding phenomena, neutralize the microcracks that cause the healing and agglomeration of fine particles, play a good dispersing role, and effectively extend the grinding limit. At the same time, some chemical substances also react chemically with aluminum, silicon, calcium, etc. in cement to produce intermediate substances with enhancement functions, and at the same time cause oxide lattice defects in cement, increase cement activity, thereby improving cement strength and improving cement performance;
[0032] The cement grinding-aiding and reinforcing powder prepared by the invention can reduce energy consumption, has a grinding-aiding effect on cement powder, improves the dispersibility of cement, has a certain early strength effect on the produced cement, improves the strength of cement, and at the same time, has a promoting effect on cement mineral hydration, and can improve the comprehensive performance of cement. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The nano-silicon dioxide used in the following examples has an average particle size of 100±10 nm and was purchased from Hubei Huifu Nanomaterials Co., Ltd.
[0035] Example 1
[0036] This embodiment provides a method for preparing cement grinding aid and enhancement powder, comprising the following steps:
[0037] S1. Polydopamine coating: 10 g of nano-silica was added to 200 mL of water, 12 g of dopamine hydrochloride and 1 g of catalyst, heated to 45°C, stirred for 2 h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0038] The catalyst is a Tris-HCl solution with a pH of 8.5;
[0039] S2. Preparation of modified nano-silica: 10 g of the polydopamine-modified nano-silica prepared in step S1 was added to 100 mL of ethanol, 2 g of silane coupling agent KH570 was added, heated to 40 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0040] S3 preparation of hyperbranched nanoparticles: 10g of the modified nano-silica prepared in step S2 was added to 200mL of xylene, 7g of dimethylol propionic acid, 0.07g of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 5h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0041] S4 Preparation of inorganic salt: 1g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0042] S5. Preparation of cement grinding aid enhancing powder: 5 g of acrylic acid, 2 g of isopentenyl polyoxyethylene ether, 1 g of maleic anhydride and 8 g of the hyperbranched nanoparticles prepared in step S3 were added to 200 mL of water, and under nitrogen protection, 0.01 g of the initiator system was added, heated to 55 ° C, stirred for 3 h, the product was filtered, washed, dried, and mixed with 1 g of the inorganic salt prepared in step S4, ball milled for 1 h, and dried to obtain cement grinding aid enhancing powder;
[0043] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 3:2.
[0044] Example 2
[0045] This embodiment provides a method for preparing cement grinding aid and enhancement powder, comprising the following steps:
[0046] S1. Polydopamine coating: 10 g of nano-silica was added to 200 mL of water, 15 g of dopamine hydrochloride and 2 g of catalyst were added, heated to 55°C, stirred for 4 h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0047] The catalyst is a Tris-HCl solution with a pH of 9.5;
[0048] S2. Preparation of modified nano-silica: 10 g of the polydopamine-modified nano-silica prepared in step S1 was added to 100 mL of ethanol, 3 g of silane coupling agent A171 was added, heated to 50 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0049] S3 preparation of hyperbranched nanoparticles: 15g of the modified nano-silica prepared in step S2 was added to 200mL of xylene, 10g of dimethylol propionic acid, 0.1g of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 7h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0050] S4 Preparation of inorganic salt: 2g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0051] S5. Preparation of cement grinding enhancement powder: 7g of acrylic acid, 3g of isopentenyl polyoxyethylene ether, 2g of maleic anhydride and 12g of the hyperbranched nanoparticles prepared in step S3 were added to 200mL of water, and under nitrogen protection, 0.02g of the initiator system was added, heated to 65°C, stirred for 5h, the product was filtered, washed, dried, and mixed with 2g of the inorganic salt prepared in step S4, ball milled for 3h, and dried to obtain cement grinding enhancement powder;
[0052] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 5:2.
[0053] Example 3
[0054] This embodiment provides a method for preparing cement grinding aid and enhancement powder, comprising the following steps:
[0055] S1. Polydopamine coating: 10 g of nano-silica was added to 200 mL of water, 13.5 g of dopamine hydrochloride and 1.5 g of catalyst were added, heated to 50°C, stirred for 3 h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0056] The catalyst is a Tris-HCl solution with a pH of 9;
[0057] S2. Preparation of modified nano-silica: 10 g of the polydopamine-modified nano-silica prepared in step S1 was added to 100 mL of ethanol, 2.5 g of a silane coupling agent KH570 was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0058] S3 Preparation of hyperbranched nanoparticles: 12g of the modified nano-silica prepared in step S2 was added to 200mL of xylene, 8.5g of dimethylol propionic acid, 0.085g of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 6h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0059] S4 Preparation of inorganic salt: 1.5g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0060] S5. Preparation of cement grinding enhancement powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, 1.5 g of maleic anhydride and 10 g of the hyperbranched nanoparticles obtained in step S3 were added to 200 mL of water, and under nitrogen protection, 0.015 g of the initiator system was added, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, and mixed with 1.5 g of the inorganic salt obtained in step S4, ball milled for 2 h, and dried to obtain cement grinding enhancement powder;
[0061] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0062] Comparative Example 1
[0063] Compared with embodiment 3, the difference is that the method of step S1 is different.
[0064] The details are as follows:
[0065] S1. Preparation of amino-modified nano-silica: 10 g of nano-silica was added to 200 mL of water, 15 g of silane coupling agent KH550 was added, the mixture was heated to 50° C., stirred for 3 h, centrifuged, washed, and dried to obtain amino-modified nano-silica;
[0066] S2. Preparation of modified nano-silica: 10 g of the amino-modified nano-silica obtained in step S1 was added to 100 mL of ethanol, 2.5 g of silane coupling agent KH570 was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0067] S3 Preparation of hyperbranched nanoparticles: 12g of the modified nano-silica prepared in step S2 was added to 200mL of xylene, 8.5g of dimethylol propionic acid, 0.085g of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 6h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0068] S4 Preparation of inorganic salt: 1.5g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0069] S5. Preparation of cement grinding enhancement powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, 1.5 g of maleic anhydride and 10 g of the hyperbranched nanoparticles obtained in step S3 were added to 200 mL of water, and under nitrogen protection, 0.015 g of the initiator system was added, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, and mixed with 1.5 g of the inorganic salt obtained in step S4, ball milled for 2 h, and dried to obtain cement grinding enhancement powder;
[0070] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0071] Comparative Example 2
[0072] Compared with Example 3, the difference is that step S1 is not performed.
[0073] The details are as follows:
[0074] S1. Preparation of modified nano-silica: 10 g of nano-silica was added to 100 mL of ethanol, 2.5 g of silane coupling agent KH570 was added, the mixture was heated to 45°C, stirred for reaction for 2 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0075] S2 Preparation of hyperbranched nanoparticles: 12g of the modified nano-silica prepared in step S2 was added to 200mL of xylene, 8.5g of dimethylol propionic acid, 0.085g of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 6h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0076] S3 Preparation of inorganic salt: 1.5g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0077] S4. Preparation of cement grinding enhancement powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, 1.5 g of maleic anhydride and 10 g of the hyperbranched nanoparticles prepared in step S2 were added to 200 mL of water, and under nitrogen protection, 0.015 g of the initiator system was added, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, and mixed with 1.5 g of the inorganic salt prepared in step S3, ball milled for 2 h, and dried to obtain cement grinding enhancement powder;
[0078] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0079] Comparative Example 3
[0080] Compared with Example 3, the difference is that step S2 is not performed.
[0081] The details are as follows:
[0082] S1. Polydopamine coating: 10 g of nano-silica was added to 200 mL of water, 13.5 g of dopamine hydrochloride and 1.5 g of catalyst were added, heated to 50°C, stirred for 3 h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0083] The catalyst is a Tris-HCl solution with a pH of 9;
[0084] S2. Preparation of hyperbranched nanoparticles: 12 g of the polydopamine-modified nanosilica prepared in step S1 was added to 200 mL of xylene, 8.5 g of dimethylolpropionic acid, 0.085 g of p-toluenesulfonic acid were added, the reaction was heated under reflux with stirring for 6 h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0085] S3 Preparation of inorganic salt: 1.5g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0086] S4. Preparation of cement grinding enhancement powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, 1.5 g of maleic anhydride and 10 g of the hyperbranched nanoparticles prepared in step S2 were added to 200 mL of water, and under nitrogen protection, 0.015 g of the initiator system was added, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, and mixed with 1.5 g of the inorganic salt prepared in step S3, ball milled for 2 h, and dried to obtain cement grinding enhancement powder;
[0087] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0088] Comparative Example 4
[0089] Compared with Example 3, the difference is that step S3 is not performed.
[0090] The details are as follows:
[0091] S1. Polydopamine coating: 10 g of nano-silica was added to 200 mL of water, 13.5 g of dopamine hydrochloride and 1.5 g of catalyst were added, heated to 50°C, stirred for 3 h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0092] The catalyst is a Tris-HCl solution with a pH of 9;
[0093] S2. Preparation of modified nano-silica: 10 g of the polydopamine-modified nano-silica prepared in step S1 was added to 100 mL of ethanol, 2.5 g of a silane coupling agent KH570 was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0094] S3 Preparation of inorganic salt: 1.5g of sodium chloride and 10g of sodium tripolyphosphate were stirred and mixed for 10min to obtain an inorganic salt;
[0095] S4. Preparation of cement grinding enhancement powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, 1.5 g of maleic anhydride and 10 g of modified nano-silica obtained in step S2 were added to 200 mL of water, and under nitrogen protection, 0.015 g of the initiator system was added, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, and mixed with 1.5 g of the inorganic salt obtained in step S3, ball milled for 2 h, and dried to obtain cement grinding enhancement powder;
[0096] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0097] Comparative Example 5
[0098] Compared with Example 3, the difference is that the inorganic salt in step S4 is single sodium chloride.
[0099] Comparative Example 6
[0100] Compared with Example 3, the difference is that the inorganic salt in step S4 is a single sodium tripolyphosphate.
[0101] Comparative Example 7
[0102] Compared with Example 3, the difference is that no inorganic salt is added in step S5.
[0103] The details are as follows:
[0104] S1. Polydopamine coating: 10 g of nano-silica was added to 200 mL of water, 13.5 g of dopamine hydrochloride and 1.5 g of catalyst were added, heated to 50°C, stirred for 3 h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica;
[0105] The catalyst is a Tris-HCl solution with a pH of 9;
[0106] S2. Preparation of modified nano-silica: 10 g of the polydopamine-modified nano-silica prepared in step S1 was added to 100 mL of ethanol, 2.5 g of a silane coupling agent KH570 was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified nano-silica;
[0107] S3 Preparation of hyperbranched nanoparticles: 12g of the modified nano-silica prepared in step S2 was added to 200mL of xylene, 8.5g of dimethylol propionic acid, 0.085g of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 6h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles;
[0108] S4. Preparation of cement grinding aid enhancing powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, 1.5 g of maleic anhydride and 10 g of the hyperbranched nanoparticles prepared in step S3 were added to 200 mL of water, and under nitrogen protection, 0.015 g of the initiator system was added, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, ball milled for 2 h, and dried to obtain cement grinding aid enhancing powder;
[0109] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0110] Comparative Example 8
[0111] Compared with Example 3, the difference is that no hyperbranched nanoparticles are added in step S5.
[0112] The details are as follows:
[0113] S1. Preparation of inorganic salt: 1.5 g of sodium chloride and 10 g of sodium tripolyphosphate were stirred and mixed for 10 min to obtain an inorganic salt;
[0114] S2. Preparation of cement grinding enhancement powder: 6 g of acrylic acid, 2.5 g of isopentenyl polyoxyethylene ether, and 1.5 g of maleic anhydride were added to 200 mL of water, and 0.015 g of the initiator system was added under nitrogen protection, heated to 60 ° C, stirred for 4 h, the product was filtered, washed, dried, and mixed with 1.5 g of the inorganic salt obtained in step S1 and ball milled for 2 h, and dried to obtain cement grinding enhancement powder;
[0115] The initiation system comprises an initiator and sodium sulfite in a mass ratio of 4:2.
[0116] Test Example 1
[0117] The cement grinding enhancement powder prepared in Examples 1-3 and Comparative Examples 1-8 was mixed into cement (the group without addition was used as a blank group) at 0.02 wt %, ground in a Φ500 mm×500 mm standard test mill, and various physical properties of the ground cement were measured.
[0118] Cement ratio: clinker 50wt%, slag 40wt%, limestone 5wt%, gypsum (calcium sulfate dihydrate content> 95%) 5wt%.
[0119] The specific surface area of cement was measured by BT-1 Blaine specific surface area meter. The cement fineness was measured in accordance with GB / T 1345-2005 “Test method for cement fineness: sieve analysis method”.
[0120] The results are shown in Table 1.
[0121] Table 1:
[0122]
[0123] It can be seen from the above table that the cement grinding aid enhancement powder prepared in Examples 1-3 of the present invention can significantly improve the grinding aid effect, significantly reduce the 45 μm and 80 μm sieve residue values, and greatly increase the specific surface area.
[0124] Cement, standard sand and water were made into standard test pieces of 40mm×40mm×160mm in a ratio of 1:3.0:0.5, and cured under standard curing conditions, and their strengths at 3d and 28d were measured respectively. The strength of cement was tested in accordance with GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)".
[0125] The results are shown in Table 2.
[0126] Table 2:
[0127]
[0128] It can be seen from the above table that the cement grinding aid and reinforcing powder prepared in Examples 1-3 of the present invention can significantly improve the mechanical strength of cement.
[0129] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing cement grinding aid and enhancement powder, characterized in that: After polydopamine is coated on nano-silica, the surface is modified with a silane coupling agent, and then reacted with dimethylol propionic acid under the catalysis of p-toluenesulfonic acid to obtain hyperbranched nanoparticles, which are copolymerized with acrylic acid, isopentenyl polyoxyethylene ether, and maleic anhydride, filtered, washed, dried, mixed with sodium chloride and sodium tripolyphosphate, ball-milled, and dried to obtain cement grinding enhancement powder; wherein, The silane coupling agent is a silane coupling agent with double bonds, and the modification steps of the silane coupling agent include: adding polydopamine-coated nano-silicon dioxide into ethanol, adding the silane coupling agent, heating and stirring to react, centrifuging, washing, and drying.
2. The preparation method according to claim 1, characterized in that: The following steps are involved: S1. Polydopamine coating: adding nano-silica to water, adding dopamine hydrochloride and a catalyst, heating and stirring to react, centrifuging, washing, and drying to obtain polydopamine-modified nano-silica; S2. Preparation of modified nano-silica: The polydopamine-coated nano-silica obtained in step S1 was added to ethanol, a silane coupling agent was added, the reaction was heated and stirred, centrifuged, washed, and dried to obtain modified nano-silica; S3 preparation of hyperbranched nanoparticles: the modified nano-silica prepared in step S2 was added to xylene, dimethylol propionic acid, p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring, centrifuged, washed, and dried to obtain hyperbranched nanoparticles; S4. Preparation of inorganic salt: sodium chloride and sodium tripolyphosphate were mixed to obtain an inorganic salt; S5. Preparation of cement grinding aid enhancing powder: acrylic acid, isopentenyl polyoxyethylene ether, maleic anhydride and the hyperbranched nanoparticles obtained in step S3 are added to water, and under the protection of inert gas, an initiator system is added, and the reaction is heated and stirred. The product is filtered, washed, and dried, and mixed with the inorganic salt obtained in step S4, ball-milled, and dried to obtain cement grinding aid enhancing powder.
3. The preparation method according to claim 2, characterized in that: The mass ratio of the nano-silicon dioxide, dopamine hydrochloride and catalyst in step S1 is 10:(12-15):(1-2), the catalyst is a Tris-HCl solution with a pH of 8.5-9.5, the average particle size of the nano-silicon dioxide is 80-120 nm, the temperature of the heating and stirring reaction is 45-55° C., and the time is 2-4 h.
4. The preparation method according to claim 2, characterized in that: In step S2, the mass ratio of the polydopamine-modified nano-silica to the silane coupling agent is 10:(2-3), the silane coupling agent is selected from at least one of KH570, A151, and A171, and the temperature of the heating and stirring reaction is 40-50° C. and the time is 1-3 hours.
5. The preparation method according to claim 2, characterized in that: The mass ratio of modified nano-silica, dimethylolpropionic acid and p-toluenesulfonic acid in step S3 is (10-15): (7-10): (0.07-0.1), and the stirring reaction time is 5-7 hours.
6. The preparation method according to claim 2, characterized in that: The mass ratio of sodium chloride to sodium tripolyphosphate in step S4 is (1-2):
10.
7. The preparation method according to claim 2, characterized in that: In step S5, the mass ratio of acrylic acid, isopentenyl polyoxyethylene ether, maleic anhydride, hyperbranched nanoparticles, and inorganic salt is (5-7): (2-3): (1-2): (8-12): (1-2), the initiator system includes an initiator and sodium sulfite in a mass ratio of (3-5): 2, the initiator is selected from at least one of potassium persulfate, sodium persulfate, and ammonium persulfate, the temperature of the heating and stirring reaction is 55-65° C., the time is 3-5 hours, and the ball milling time is 1-3 hours.
8. The preparation method according to claim 2, characterized in that: The specific steps include: S1. Polydopamine coating: 10 parts by weight of nano-silica was added to water, 12-15 parts by weight of dopamine hydrochloride and 1-2 parts by weight of a catalyst were added, heated to 45-55°C, stirred for 2-4h, centrifuged, washed, and dried to obtain polydopamine-modified nano-silica; The catalyst is a Tris-HCl solution with a pH of 8.5-9.5; S2. Preparation of modified nano-silica: 10 parts by weight of the polydopamine-modified nano-silica prepared in step S1 was added to ethanol, 2-3 parts by weight of a silane coupling agent was added, heated to 40-50 ° C, stirred for 1-3h, centrifuged, washed, and dried to obtain modified nano-silica; S3 preparation of hyperbranched nanoparticles: 10-15 parts by weight of the modified nano-silica obtained in step S2 was added to xylene, 7-10 parts by weight of dimethylol propionic acid, 0.07-0.1 parts by weight of p-toluenesulfonic acid were added, the reaction was heated to reflux with stirring for 5-7h, centrifuged, washed, and dried to obtain hyperbranched nanoparticles; S4 Preparation of an inorganic salt: 1-2 parts by weight of sodium chloride, 10 parts by weight of sodium tripolyphosphate were stirred and mixed to obtain an inorganic salt; S5. Preparation of cement grinding aid enhancing powder: 5-7 parts by weight of acrylic acid, 2-3 parts by weight of isopentyl polyoxyethylene ether, 1-2 parts by weight of maleic anhydride and 8-12 parts by weight of the hyperbranched nanoparticles obtained in step S3 are added to water, under inert gas protection, 0.01-0.02 parts by weight of the initiator system is added, heated to 55-65 ° C, stirred for 3-5h, the product is filtered, washed, dried, and mixed with 1-2 parts by weight of the inorganic salt obtained in step S4 and ball milled for 1-3h, dried to obtain cement grinding aid enhancing powder; The initiation system comprises an initiator and sodium sulfite in a mass ratio of 3-5:
2.
9. A cement grinding aid and enhancement powder obtained by the preparation method according to any one of claims 1 to 8.