A method for improving the performance of prebaked carbon anode for aluminum
By using high-conductive filler inlay technology in aluminum electrolytic prebaked carbon anode, the pore problem of petroleum coke is solved, density and conductive properties are improved, pollution and production costs are reduced, and energy saving and emission reduction of aluminum electrolysis is achieved.
Patent Information
- Application Number
- CN202411017185.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the existing aluminum electrolytic prebaked carbon anode production process, there are 30% to 55% pores after calcination of petroleum coke, which makes it difficult to improve performance indicators such as conductivity and strength, and asphalt consumes a lot and produces harmful gases. The resistance during electrolysis is It is difficult to reduce, resulting in high energy consumption and high greenhouse gas emissions.
Using high-conductivity pollution-free fillers (such as graphite) are embedded in the calcined petroleum coke particles through filling micropore technology, combined with suitable production process control, bonding with asphalt or resin to form high-performance prebaking Carbon anode.
It effectively fills the pores of petroleum coke, improves the density and conductivity of the carbon anode, reduces pollution, reduces production costs and electrolytic pressure drop, and realizes energy-saving and emission reduction of aluminum electrolysis.
Smart Images

Figure CN118545999B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy saving in aluminum electrolysis and production of carbon anodes, and in particular to a method for improving the performance of prebaked carbon anodes for aluminum. Background Art
[0002] Prebaked carbon anodes are essential materials for prebaked aluminum reduction cells, often called the "heart" of the cell. They function as both conductors and direct participants in the electrochemical reaction during the aluminum electrolysis process. They are manufactured using calcined petroleum coke of varying particle sizes as aggregate, and asphalt or resin as a binder in a specific ratio through a series of processes including mixing, forming, and calcining to produce carbon anodes of varying specifications to meet the needs of aluminum electrolysis production.
[0003] At present, the production process technology commonly used in the world for aluminum prebaked anodes has the following major problems: First, petroleum coke generally has 30% to 55% porosity after high-temperature calcination, which seriously affects the density, conductivity, strength, etc. of the product; Second, to solve the porosity problem of calcined coke, the only solution currently in the world is to use asphalt for a long time to knead it so that the asphalt can fully penetrate the pores of the calcined petroleum coke. After high-temperature calcination, the asphalt is cracked into carbon and retained in the aggregate. However, during the calcination process, less than 50% of the asphalt is carbonized, resulting in a large secondary porosity in the aggregate and inside the carbon anode. This problem has not been effectively solved, making it difficult to effectively improve the key performance indicators of the carbon anode, such as resistivity and density; Fourth, the consumption of asphalt or resin is high. Asphalt and resin are both serious pollutants, and a large amount of harmful gases such as asphalt smoke are generated during the calcination process. Fourth, the main performance indicators of aluminum prebaked anodes have remained at: volume density of 1.52 g / cm3 to 1.55 g / cm3, resistivity of 52μΩ.m to 57 μΩ.m, which has not been effectively improved for a long time; fifthly, in the process of electrolytic aluminum, because its carbon anode resistivity cannot be effectively reduced, the carbon anode voltage drop in the process of electrolytic aluminum cannot be effectively reduced, and the process of electrolytic aluminum always maintains high energy consumption and high greenhouse gas emissions. Summary of the Invention
[0004] The purpose of the present invention is to provide a method for improving the performance of prebaked carbon anodes for aluminum. By adopting a pollution-free filler with high conductivity and through appropriate micropore filling technology and production process control, graphite or calcined petroleum coke with excellent performance is "embedded" in the internal cavities of calcined petroleum coke particles, effectively filling 30% to 55% of the pores generated by the petroleum coke used in the production of prebaked carbon anodes for aluminum after calcination.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for improving the performance of prebaked carbon anodes for aluminum, comprising the steps of:
[0007] S1. preparing a non-polluting filler with high electrical conductivity, using large-particle calcined petroleum coke and medium-particle calcined petroleum coke to fill the non-polluting filler with high electrical conductivity into the internal pores of the calcined petroleum coke aggregate to obtain an aggregate with the filler;
[0008] S2. Place 16-20 parts of calcined petroleum coke with a particle size of 1-3 mm as fine material, 35-40 parts of calcined petroleum coke with a particle size of less than 1 mm as powder material, and 30-45 parts of aggregate with filler in a preheated kneading pot and preheat and knead for 10-25 minutes;
[0009] S3, adding 82-92 parts of the preheated aggregate with filler prepared by mixing and kneading 8-18 parts of liquid asphalt or resin and kneading at 160° C. to 185° C., kneading for 25-45 minutes and then cooling the material under uninterrupted kneading, and feeding the cooled material into a vibration molding machine or a vacuum vibration molding machine for vibration molding to produce biochar anode blocks;
[0010] S4. The biochar anode block is baked in a baking furnace. The filler and the binder are well sintered with the aggregate during the high-temperature carbonization process to form a pre-baked carbon anode with better conductivity and effectively increased density.
[0011] Preferably, the filler comprises: graphite tailings with a particle size of 1 to 6.5 μm produced in the production of lithium battery negative electrodes, and graphite with a particle size of 1 to 6.5 μm.
[0012] Preferably, the particle size of the large-particle calcined petroleum coke is 6 to 18 mm, and the particle size of the medium-particle calcined petroleum coke is 3 to 6 mm.
[0013] Preferably, the step of filling the filler into the internal pores of the calcined petroleum coke aggregate comprises:
[0014] 10 to 15 parts of the large-particle calcined petroleum coke and 0.5 to 2.5 parts of the filler are mixed in a kneading pot at room temperature for 10 to 40 minutes; the filler is fully absorbed into the internal pores of the calcined petroleum coke aggregate by making full use of the adsorption effect of the abundant pores of the large-particle calcined petroleum coke, the stirring power, and the gravity of the material in the kneading pot;
[0015] 20 to 25 parts of the medium-sized calcined petroleum coke and 0.5 to 2.0 parts of the filler are added to a kneading pot of the previously mixed large-sized calcined petroleum coke at room temperature and mixed for 10 to 30 minutes to fill the gaps between the large-sized and medium-sized calcined petroleum coke particles.
[0016] Preferably, the preheating temperature is controlled at 160°C to 190°C, and during the preheating and kneading process, asphalt or resin is used to consolidate the filler into the internal pores of the calcined petroleum coke aggregate, and asphalt or resin is used to fill the remaining capillary pores of the calcined petroleum coke as much as possible, while bonding aggregates of various particle sizes together.
[0017] Preferably, the cooling temperature during the uninterrupted kneading process is 155°C ± 5°C to ensure uniformity of the liquid asphalt or resin and the aggregate.
[0018] Preferably, the vibration molding temperature of the vibration molding machine or vacuum vibration molding machine is controlled between 150° C. and 160° C., and the vibration molding time is 60 to 80 seconds.
[0019] Preferably, the biochar anode block is roasted in a roasting furnace for 168 to 208 hours, the high temperature zone of the roasting is controlled at 1150° C. to 1250° C., and the high temperature zone is maintained for 7.5 to 8.5 hours.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: by adopting pollution-free fillers with high electrical conductivity, and through appropriate filling micropore technology and production process control, graphite or calcined petroleum coke with excellent performance is "embedded" in the internal cavities of calcined petroleum coke particles, effectively filling 30% to 55% of the pores produced by calcination of petroleum coke used in the production of prebaked anodes for aluminum, effectively changing the secondary pores produced by calcination after the original asphalt filling, etc., comprehensively improving the key performance indicators of the prebaked carbon anode for aluminum, such as resistivity and density, and effectively reducing pollution; at the same time, larger particles of calcined petroleum coke can be used, effectively reducing the workload of screening and crushing, reducing production costs; reducing the anode pressure of the aluminum electrolytic cell; not only breaking the long-term problem of difficulty in improving the performance indicators of prebaked carbon anodes for aluminum, but also laying an effective and reliable guarantee for energy conservation and emission reduction of electrolytic aluminum, having strong practicality and wide applicability, and generating significant economic and social benefits for the electrolytic aluminum industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0022] Figure 1 This is a flow chart of the steps of a method for improving the performance of prebaked carbon anodes for aluminum according to the present invention;
[0023] Figure 2 It is a comparison diagram of the cross section of a product produced by a traditional method and a finished product produced by the technology of the present invention. DETAILED DESCRIPTION
[0024] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0025] Example 1 Preparation of 200×150×100 mm carbon anode block
[0026] Graphite tailings produced from the production of lithium battery negative electrodes with a particle size of 1 to 6.5 μm are used as fillers;
[0027] First, 12 parts of calcined petroleum coke with a large particle size of 6 to 18 mm and 1.5 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are mixed in a kneading pot at room temperature for 30 minutes. The graphite powder is fully absorbed into the internal pores of the calcined petroleum coke by making full use of the adsorption effect of the rich pores of the large particle calcined petroleum coke, the stirring power and the gravity of the material in the kneading pot.
[0028] Then, 20 parts of calcined petroleum coke with a medium particle size of 3 to 6 mm and 0.8 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are added to the previously mixed large particle kneading pot at room temperature and mixed for 20 minutes;
[0029] Then, 18 parts of calcined petroleum coke with a fine particle size of 1 to 3 mm, 37 parts of calcined petroleum coke with a powder particle size of less than 1 mm, and 30.2 parts of the aggregate mixed with fillers in the previous order are placed in a preheating kneading pot for preheating (temperature controlled at 175°C) and kneaded for 20 minutes. Then, 14.8 parts of liquid asphalt are added and kneaded at 165°C. After kneading for 35 minutes, the material is cooled to 155°C without stopping kneading. The material is placed in a vibration molding machine mold and vibrated for 62 seconds to produce a biochar block. The biochar block is roasted in a roasting furnace for 192 hours with a maximum roasting temperature of 1250°C. It is kept in the maximum roasting temperature zone for 8 hours and then naturally cooled. The volume density of the obtained carbon block reaches 1.61g / cm 3 , the resistivity reaches 49.65μΩ.m, and the asphalt consumption is saved by 1.2kg / t compared with traditional production.
[0030] Example 2: Preparation of prebaked carbon anodes for 400kA prebaked aluminum electrolytic cells, with specifications of 1650×700×620mm.
[0031] Graphite tailings produced from the production of lithium battery negative electrodes with a particle size of 1 to 6.5 μm are used as fillers;
[0032] First, 15 parts of calcined petroleum coke with a large particle size of 6 to 18 mm and 1.5 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are mixed in a kneading pot at room temperature for 30 minutes. The graphite powder is fully absorbed into the internal pores of the calcined petroleum coke by making full use of the adsorption effect of the rich pores of the large particle calcined petroleum coke, the stirring power and the gravity of the material in the kneading pot.
[0033] Then, 20 parts of calcined petroleum coke with a medium particle size of 3 to 6 mm and 0.8 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are added to the previously mixed large particle kneading pot at room temperature and mixed for 20 minutes;
[0034] Then, 16 parts of calcined petroleum coke with a fine particle size of 1 to 3 mm, 40 parts of calcined petroleum coke with a powder particle size less than 1 mm and 29 parts of aggregate with fillers mixed in the previous order are placed in a preheating kneading pot for preheating (temperature controlled at 175°C) and kneaded for 20 minutes. Then, 15 parts of liquid asphalt are added and kneaded at 165°C. After kneading for 35 minutes, the material is cooled to 155°C without stopping kneading. The material is placed in a vibration molding machine mold and vibrated for 60 seconds to produce a biochar block. The biochar block is roasted in a roasting furnace for 192 hours with a maximum roasting temperature of 1250°C. It is kept in the maximum roasting temperature zone for 8 hours, and then forced cooling and natural cooling are adopted. The volume density of the obtained carbon block reaches 1.60g / cm 3 , the resistivity reaches 50.16μΩ.m, and the asphalt consumption is saved by 1.0kg / t compared with traditional production.
[0035] Example 3: Preparation of a prebaked carbon anode block for a 500kA prebaked aluminum electrolytic cell with a specification of 1750×740×620mm
[0036] Graphite tailings produced from the production of lithium battery negative electrodes with a particle size of 1 to 6.5 μm are used as fillers;
[0037] First, 15 parts of calcined petroleum coke with a large particle size of 6 to 18 mm and 1.5 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are mixed in a kneading pot at room temperature for 30 minutes. The adsorption effect of the rich pores of the large particle calcined petroleum coke itself, the stirring power and the gravity of the material in the kneading pot are fully utilized to allow the graphite powder to fully enter the internal pores of the calcined petroleum coke.
[0038] Then, 22 parts of calcined petroleum coke with a medium particle size of 3 to 6 mm and 1 part of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are added to the previously mixed large particle kneading pot at room temperature and mixed for 20 minutes;
[0039] Then, 18 parts of calcined petroleum coke with a fine particle size of 1 to 3 mm, 37 parts of calcined petroleum coke with a powder particle size of less than 1 mm and 30 parts of the aggregate mixed with fillers in the previous order are placed in a preheating kneading pot for preheating (temperature controlled at 175°C) and kneaded for 20 minutes. After that, 15 parts of liquid asphalt are added and kneaded at 165°C for 35 minutes. After kneading for 35 minutes, the material is cooled to 155°C without stopping kneading. The material is placed in a vibration molding mold and vibrated for 62 seconds to produce a biochar block. The biochar block is roasted in a roasting furnace for 208 hours with a maximum roasting temperature of 1250°C. It is kept in the maximum roasting temperature zone for 7.5 hours, and then forced cooling and natural cooling are adopted. The volume density of the obtained carbon block reaches 1.61g / cm 3 , the resistivity reaches 50.25μΩ.m, and the asphalt consumption is saved by 1.0kg / t compared with traditional production.
[0040] Example 4: Preparation of a prebaked carbon anode block for a 600kA prebaked aluminum electrolytic cell with a size of 1750×750×680 mm
[0041] Graphite tailings produced from the production of lithium battery negative electrodes with a particle size of 1 to 6.5 μm are used as fillers;
[0042] First, 13 parts of calcined petroleum coke with a large particle size of 6 to 15 mm and 1.2 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are mixed in a kneading pot at room temperature for 30 minutes. The graphite powder is fully absorbed into the internal pores of the calcined petroleum coke by making full use of the adsorption effect of the rich pores of the large particle calcined petroleum coke, the stirring power and the gravity of the material in the kneading pot.
[0043] Then, 18 parts of calcined petroleum coke with a medium particle size of 3 to 6 mm and 0.8 parts of a prepared graphite filler with a particle size of 1 to 6.5 μm and high conductivity are added to the previously mixed large particle kneading pot at room temperature and mixed for 10 to 30 minutes;
[0044] Then, 17 parts of calcined petroleum coke with a fine particle size of 1 to 3 mm, 38 parts of calcined petroleum coke with a powder particle size of less than 1 mm, and 30 parts of the aggregate with fillers mixed in the previous order are placed in a preheating kneading pot for preheating (temperature controlled at 175°C) and kneaded for 20 minutes. Then, 15 parts of liquid asphalt are added and kneaded at 165°C. After kneading for 35 minutes, the material is cooled to 155°C without stopping kneading. The material is placed in a vibration molding mold and vibrated for 61 seconds to produce a biochar block. The biochar block is roasted in a roasting furnace for 192 hours with a maximum roasting temperature of 1250°C. It is kept in the maximum roasting temperature zone for 8 hours, and then forced cooling and natural cooling are adopted. The volume density of the obtained carbon block reaches 1.61g / cm 3, the resistivity reaches 49.86μΩ.m, and the asphalt consumption is saved by 1.0kg / t compared with traditional production.
[0045] In summary, the volume density of the aluminum prebaked carbon anode produced by the technical method of the present invention reaches 1.59g / cm 3 ~1.61 g / cm 3 The volume density of the anode is increased by 3% to 5% compared with the traditional technical method; the resistivity reaches 50μΩ.m to 53 μΩ.m; the resistivity can be reduced by 2% to 5%; each ton of carbon anode saves 1kg±0.5 kg of asphalt; it improves the performance indicators of prebaked carbon anodes for aluminum, and lays an effective and reliable guarantee for energy conservation and emission reduction of electrolytic aluminum. Taking a 600kA prebaked aluminum electrolysis production plant with an annual output of 500,000 tons as an example, it can save about 17.5 million kWh of electricity annually and reduce asphalt smoke emissions by 16,500 tons, which has significant economic and social benefits.
[0046] Figure 2 The left picture in the middle is a cross section of a product produced using traditional methods. Figure 2 The cross section of the finished product produced by the technology of the present invention is shown in the figure on the right. Figure 2 It can be seen that the present invention effectively fills the pores generated after calcination of petroleum coke used in the production of pre-baked anodes for aluminum, and effectively changes the secondary pores generated by calcination after the original asphalt filling.
[0047] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.
[0048] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art will be able to modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A method for improving the performance of prebaked carbon anode for aluminum, characterized in that: The steps include: A non-polluting filler with high conductivity is prepared by filling the non-polluting filler with high conductivity into the internal pores of the calcined petroleum coke aggregate using large-particle calcined petroleum coke and medium-particle calcined petroleum coke to obtain an aggregate with filler; the filler comprises: graphite tailings with a particle size of 1 to 6.5 μm produced by the production of lithium battery negative electrodes, and graphite with a particle size of 1 to 6.5 μm; The step of filling the filler into the internal pores of the calcined petroleum coke aggregate comprises: Mixing 10 to 15 parts of large-particle calcined petroleum coke and 0.5 to 2.5 parts of the filler in a kneading pot at room temperature for 10 to 40 minutes; 20-25 parts of medium-sized calcined petroleum coke and 0.5-2.0 parts of the filler are added to a kneading pot of the previously mixed large-sized calcined petroleum coke at room temperature and mixed for 10-30 minutes to fill the gaps between the large-sized and medium-sized calcined petroleum coke particles; Put 16-20 parts of calcined petroleum coke with a particle size of 1-3 mm, 35-40 parts of calcined petroleum coke with a particle size of less than 1 mm, and 30-45 parts of aggregate with filler in a preheating kneading pot for preheating and kneading for 10-25 minutes; 82-92 parts of aggregate with filler prepared by preheating and kneading are added with 8-18 parts of liquid asphalt or resin and kneaded at 160-185°C. After kneading for 25-45 minutes, the material is cooled under uninterrupted kneading, and the cooled material is loaded into a vibration molding machine or a vacuum vibration molding machine for vibration molding to produce a biochar anode block; The biochar anode block is roasted in a roasting furnace to obtain a pre-baked carbon anode.
2. A method for improving the performance of prebaked carbon anode for aluminum according to claim 1, characterized in that: The particle size of the large-particle calcined petroleum coke is 6 to 18 mm, and the particle size of the medium-particle calcined petroleum coke is 3 to 6 mm.
3. A method for improving the performance of prebaked carbon anode for aluminum according to claim 1, characterized in that: The preheating temperature is controlled at 160°C to 190°C.
4. A method for improving the performance of prebaked carbon anode for aluminum according to claim 1, characterized in that: The cooling temperature during the uninterrupted kneading process is 155°C ± 5°C.
5. A method for improving the performance of prebaked carbon anode for aluminum according to claim 1, characterized in that: The vibration molding temperature of the vibration molding machine or the vacuum vibration molding machine is controlled between 150° C. and 160° C., and the vibration molding time is 60 to 80 seconds.
6. A method for improving the performance of prebaked carbon anode for aluminum according to claim 1, characterized in that: The biochar anode block is roasted in a roasting furnace for 168 to 208 hours, the high temperature zone of the roasting is controlled at 1150° C. to 1250° C., and the high temperature zone is maintained for 7.5 to 8.5 hours.