A reinforced toughened polymer polyol and its synthesis process
By introducing ester bonds, amino and benzene rings into polymer polyols, increasing crosslinking density and intermolecular action, the problem of the material becoming brittle after crosslinking of polymer polyols is solved, and better resistance to tear is achieved Performance and physical performance.
Patent Information
- Application Number
- CN202411020974.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing polymer polyols cause foam materials to become brittle after crosslinking and have poor tensile tear resistance.
By introducing functional groups of ester bonds, amino groups and/or benzene rings, increasing the crosslinking density and intermolecular forces of the polymer, a specific synthesis process is used to prepare toughened polymer polyols, including the base polyether group, using a specific synthesis process. and styrene-acrylonitrile copolymer components.
It effectively improves the toughness and tear resistance of polyurethane materials, while maintaining the strength and other physical properties of the material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sponge materials, and in particular relates to a reinforced and toughened polymer polyol and a synthesis process thereof. Background Art
[0002] Polymer polyol (POP) is made by grafting acrylonitrile (AN) and styrene (SM) with basic polyether (PPG) as the matrix. It is a blend system composed of copolymers or self-polymers of basic polyether, grafted basic polyether (macromolecular dispersant), styrene and vinyl monomers such as acrylonitrile. Grafted basic polyether is usually an amphiphilic polymer with interface protection, in which the hydrophobic vinyl polymer chain segment has some special affinity for the dispersed polymer and can be adsorbed or bonded to the surface of suspended solid particles in the POP system; while the hydrophilic polyether chain segment is dissolved in the basic polyether, forming a protective barrier around the continuous phase of the polyether to avoid adhesion, aggregation and sedimentation between polymer particles, playing a steric stabilization role. POP is an important type of polyol used in molding, block soft and semi-rigid polyurethane foam plastics (such as sponges).
[0003] Polyurethane foams made from polyols containing POP have cross-linked structures that can enhance the mechanical properties of polyurethane foams and are usually used as hardening components. However, due to the poor elasticity and toughness of the molecular chains of POP itself, cross-linking will cause the foam material to become brittle and its tensile and tearing resistance to deteriorate. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a reinforced and toughened polymer polyol capable of improving the tear resistance of sponge and a synthesis process thereof.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: the reinforced and toughened polymer polyol comprises a basic polyether component and a styrene-acrylonitrile copolymer component, the polyether molecular chain of the basic polyether component is connected with a side chain with an ester bond or / and a benzene ring; the molecular chain of the styrene-acrylonitrile copolymer is connected with a side chain with an ester bond and a benzene ring or a side chain with an ester bond and a tertiary amine group.
[0006] The reinforced and toughened polymer polyol of the present invention introduces ester bonds, amino groups and / or benzene rings. These functional groups increase the crosslinking density and intermolecular forces of the polymer, can effectively improve the toughness of the synthesized polyurethane material, and have better tear resistance.
[0007] A synthesis process of the above-mentioned reinforced toughened polymer polyol, the process steps are:
[0008] 1) Adding a polyol initiator, a composite epoxy compound and a catalyst into a reaction kettle, heating the reaction kettle to 40°C to 60°C and reacting the reaction kettle for 5h to 12h to prepare a basic polyether polyol, wherein the composite epoxy compound contains at least one epoxy compound containing an ester bond or an epoxy compound containing a benzene ring;
[0009] 2) Add AN, SM, modified monomer, initiator, basic polyether polyol, macromolecular dispersant and chain transfer agent into the reactor, react at 115℃~125℃, control the pressure at 0.1MPa~0.5MPa, and the reaction time is 0.5h~2.0h;
[0010] 3) Distill out the remaining monomers in the crude POP and collect the refined POP.
[0011] The synthesis process of the reinforced toughened polymer polyol of the present invention increases the crosslinking density and intermolecular force (hydrogen bond) of the polymer by introducing ester bonds, amino groups and / or benzene rings into the polymerized monomers, thereby effectively improving the tear resistance of the material. The preparation process of the basic polyether polyol can ensure the completeness and uniformity of the reaction, avoid thermal decomposition during the reaction and reduce side reactions. The POP prepared by the synthesis process of the present invention improves the toughness of the molecular chains of each component; after being used in the synthesis of foam materials, it can effectively improve the tear resistance and other physical properties of the foam while ensuring the strength of the polyurethane material.
[0012] In the above synthesis process, preferably, the epoxy compound containing an ester bond in step 1) includes glycidyl acetate, glycidyl butyrate, glycidyl acrylate, glycidyl neodecanoate or glycidyl palmitate. By introducing a side chain containing an ester bond into the base polyether through the epoxy compound, the toughness of the polyether component can be improved.
[0013] In the above synthesis process, preferably, the epoxy compound containing a benzene ring in step 1) includes 2-phenyl-1,2-epoxypropane or styrene oxide. By introducing a side chain containing a benzene ring into the base polyether through the epoxy compound, the strength of the polyether component can be improved.
[0014] In the above synthesis process, preferably, in step 1), the molar ratio of the polyol initiator, the composite epoxy compound and the catalyst is 10ː500~800ː0.01~0.1, wherein the proportion of the epoxy compound containing ester bonds and / or the epoxy compound containing benzene rings in the composite epoxy compound is 5mol%~50mol%. While maintaining a reasonable degree of polymerization of the polyether, the toughness and strength properties of the material can be adjusted by adjusting the content of the two special epoxy compounds. Too many special epoxy compounds will affect the progress of the polyether polymerization reaction, and too many side reactions will make it impossible to guarantee the molecular weight of the polyether.
[0015] More preferably, the proportion of epoxy compounds containing ester bonds in the composite epoxy compound is 5 mol% to 15 mol%, and the proportion of epoxy compounds containing benzene rings is 2 mol% to 10 mol%. Under the preferred ratio, the POP of the present invention with the best toughness and strength can be obtained, and the obtained polyurethane has the best tear resistance.
[0016] In the above synthesis process, preferably, the catalyst described in step 1) is a DMC catalyst. In the preparation of the base polyether, because the introduction of epoxy compounds containing ester bonds and epoxy compounds containing benzene rings increases the side reactions, a DMC catalyst is selected, preferably a porous composite metal catalyst described in patent 2024103918663, which has better selectivity for the above reaction polyether reaction.
[0017] In the above synthesis process, preferably, the modified monomer in step 2) is benzyl acrylate or 2-methylstyrene acrylate.
[0018] In the above synthesis process, preferably, the modified monomer in step 2) is dimethylaminoethyl methacrylate. The introduction of ester bonds and benzene rings into the copolymer of vinyl monomers can also improve the strength and toughness of POP materials. Furthermore, the introduction of amino groups (tertiary amines) into the copolymer can form hydrogen bonds between molecules, further improving the strength of the material.
[0019] In the above synthesis process, preferably, the initiator described in step 2) is azobisisobutyronitrile or dimethyl azobisisobutyrate. The macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate or a copolymer of propylene oxide and glycidyl acrylate. The chain transfer agent is glycerol, ethylene glycol or trimethylolpropane. The decomposition temperature of the selected initiator is moderate, and free radicals can be stably generated under the reaction conditions while avoiding side reactions caused by excessively high temperatures. The molar ratio of ethylene oxide to glycidyl acrylate in the comonomer of the copolymer of ethylene oxide and glycidyl acrylate is 60~70ː30~40. The molar ratio of propylene oxide to glycidyl acrylate in the comonomer of the copolymer of propylene oxide and glycidyl acrylate is 55~70ː30~45. Controlling the grafting density of the macromolecular dispersant can better play a steric stabilizing role. The selection of these chain transfer agents is conducive to obtaining polymers with moderate molecular weight and narrow molecular weight distribution, thereby improving the mechanical properties and processing properties of the polymer.
[0020] Preferably, the molar ratio of AN, SM, modified monomer, basic polyether polyol, macromolecular dispersant and chain transfer agent in step 2) is 30~40ː20~40ː5~10ː10ː30~45ː1~10.
[0021] In the above synthesis process, in step 3), the evaporator temperature is about 100° C. and the vacuum degree is -0.098 MPa.
[0022] Compared with the prior art, the enhanced toughening polymer polyol and its synthesis process of the present invention have the following beneficial effects: the preparation process of the basic polyether polyol of the present invention can avoid thermal decomposition and reduce side reactions during the reaction while ensuring complete and uniform reactions. The POP of the present invention improves its toughness by introducing ester bonds, amino groups and / or benzene rings into the molecular chains of each component; after being used to synthesize foam materials, these groups can effectively improve the toughness of the synthesized polyurethane foam materials, making them have better tear resistance. DETAILED DESCRIPTION
[0023] The present invention is further described below in conjunction with specific embodiments, wherein Embodiment 1 is the best implementation.
[0024] Example 1
[0025] 1) Glycerol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː600ː0.01, wherein the composite epoxy compound is a composite of propylene oxide, glycidyl acetate and 2-phenyl-1,2-epoxypropane at a molar ratio of 84ː10ː6; the temperature is raised to 50°C and reacted for 8 hours to prepare a basic polyether polyol;
[0026] 2) Add AN, SM, benzyl acrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and glycerol into the reactor at a molar ratio of 35ː30ː7ː0.1ː10ː35ː5. The macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate at a molar ratio of 65ː35. The reaction is carried out at 120°C, the pressure is controlled at 0.3MPa, and the reaction time is 1.5h;
[0027] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0028] Example 2
[0029] 1) Add trimethylolpropane, a composite epoxy compound and a porous composite metal catalyst in a molar ratio of 10ː700ː0.01 into a reactor, wherein the composite epoxy compound is a composite of propylene oxide, glycidyl butyrate and styrene oxide in a molar ratio of 85ː7ː8; heat to 55°C and react for 10 hours to prepare a basic polyether polyol;
[0030] 2) Add AN, SM, 2-methyl methacrylate, dimethyl azobisisobutyrate, basic polyether polyol, macromolecular dispersant, trimethylolpropane in a molar ratio of 35ː25ː8ː0.05ː10ː40ː3 into the reactor. The macromolecular dispersant is a copolymer of propylene oxide and glycidyl acrylate in a molar ratio of 60ː40. The reaction is carried out at 120℃, the pressure is controlled at 0.3MPa, and the reaction time is 1h;
[0031] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0032] Example 3
[0033] 1) Glycerol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː600ː0.01, wherein the composite epoxy compound is a composite of propylene oxide, glycidyl acrylate and 2-phenyl-1,2-epoxypropane at a molar ratio of 84ː12ː4; the temperature is raised to 45°C and reacted for 9 hours to prepare a basic polyether polyol;
[0034] 2) Add AN, SM, dimethylaminoethyl methacrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and glycerol in a molar ratio of 32ː28ː7ː0.1ː10ː35ː8 into the reactor, wherein the macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate in a molar ratio of 70ː30. The reaction is carried out at 120°C, the pressure is controlled at 0.2MPa, and the reaction time is 1.5h;
[0035] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0036] Example 4
[0037] 1) Glycerol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː600ː0.01, wherein the composite epoxy compound is a composite of propylene oxide, glycidyl acetate and styrene oxide at a molar ratio of 85ː5ː10; the temperature is raised to 60°C and reacted for 5 hours to prepare a basic polyether polyol;
[0038] 2) Add AN, SM, dimethylaminoethyl methacrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and glycerol in a molar ratio of 30ː40ː5ː0.1ː10ː45ː1 into the reactor, wherein the macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate in a molar ratio of 60ː40. The reaction is carried out at 115°C, the pressure is controlled at 0.1MPa, and the reaction time is 2.0h;
[0039] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0040] Example 5
[0041] 1) Glycerol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː500ː0.01, wherein the composite epoxy compound is a composite of propylene oxide, glycidyl acrylate and 2-phenyl-1,2-epoxypropane at a molar ratio of 83ː15ː2; the temperature is raised to 40°C and reacted for 12 hours to prepare a basic polyether polyol;
[0042] 2) Add AN, SM, 2-methyl methacrylate, dimethyl azobisisobutyrate, basic polyether polyol, macromolecular dispersant, and trimethylolpropane in a molar ratio of 40ː20ː10ː0.05ː10ː30ː10 into the reactor, wherein the macromolecular dispersant is a copolymer of propylene oxide and glycidyl acrylate in a molar ratio of 55ː45. The reaction is carried out at 125°C, the pressure is controlled at 0.5MPa, and the reaction time is 0.5h;
[0043] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0044] Example 6
[0045] 1) Ethylene glycol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː800ː0.01, wherein the composite epoxy compound is a composite of propylene oxide and glycidyl neodecanoate at a molar ratio of 50ː50; the temperature is raised to 50°C and reacted for 8 hours to prepare a basic polyether polyol;
[0046] 2) Add AN, SM, benzyl acrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and ethylene glycol in a molar ratio of 35ː25ː7ː0.1ː10ː35ː6 into the reactor, wherein the molecular dispersant is a copolymer of glycidyl acrylate in a molar ratio of 70ː30. The reaction is carried out at 120°C, the pressure is controlled at 0.3MPa, and the reaction time is 1.2h;
[0047] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is about 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0048] Example 7
[0049] 1) Ethylene glycol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː800ː0.01, wherein the composite epoxy compound is a composite of propylene oxide and styrene oxide at a molar ratio of 95ː5; the temperature is raised to 50°C and reacted for 8 hours to prepare a basic polyether polyol;
[0050] 2) Add AN, SM, benzyl acrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and ethylene glycol in a molar ratio of 35ː25ː7ː0.1ː10ː35ː6 into the reactor, wherein the molecular dispersant is a copolymer of glycidyl acrylate in a molar ratio of 70ː30. The reaction is carried out at 120°C, the pressure is controlled at 0.3MPa, and the reaction time is 1.2h;
[0051] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is about 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0052] Comparative Example 1
[0053] 1) Add glycerol, propylene oxide and sodium methoxide into a reactor at a molar ratio of 10ː600ː0.01; heat to 50°C and react for 8 hours to prepare a basic polyether polyol;
[0054] 2) Add AN, SM, benzyl acrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and glycerol into the reactor at a molar ratio of 35ː30ː7ː0.1ː10ː35ː5. The macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate at a molar ratio of 65ː35. The reaction is carried out at 120°C, the pressure is controlled at 0.3MPa, and the reaction time is 1.5h;
[0055] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0056] Comparative Example 2
[0057] 1) Glycerol, a composite epoxy compound and a porous composite metal catalyst are added into a reactor at a molar ratio of 10ː600ː0.01, wherein the composite epoxy compound is a composite of propylene oxide, glycidyl acetate and 2-phenyl-1,2-epoxypropane at a molar ratio of 100ː10ː6; the temperature is raised to 50°C and reacted for 8 hours to prepare a basic polyether polyol;
[0058] 2) Add AN, SM, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and glycerol into the reactor at a molar ratio of 35ː30ː0.1ː10ː35ː5. The macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate at a molar ratio of 65ː35. The reaction is carried out at 120℃, the pressure is controlled at 0.3MPa, and the reaction time is 1.5h;
[0059] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0060] Comparative Example 3
[0061] 1) Add glycerol, propylene oxide and sodium methoxide into a reactor at a molar ratio of 10ː600ː0.01, heat to 50°C and react for 8 hours to prepare a basic polyether polyol;
[0062] 2) Add AN, SM, methyl acrylate, azobisisobutyronitrile, basic polyether polyol, macromolecular dispersant, and glycerol into the reactor at a molar ratio of 35ː30ː7ː0.1ː10ː35ː5. The macromolecular dispersant is a copolymer of ethylene oxide and glycidyl acrylate at a molar ratio of 65ː35. The reaction is carried out at 120℃, the pressure is controlled at 0.3MPa, and the reaction time is 1.5h;
[0063] 3) Use an evaporator to evaporate the remaining monomers in the crude POP. The evaporator temperature is 100°C and the vacuum degree is -0.098MPa, and the refined POP is collected.
[0064] 100 parts of POP obtained in each embodiment were mixed with 4 parts of water, 0.2 parts of triethanolamine and 0.8 parts of silicone oil by weight, and stirred for 20 seconds to prepare component A. Then 51 parts of TDI and 0.24 parts of organotin were stirred for 10 seconds to prepare component B. Components A and B were mixed and stirred at high speed for 10 seconds, and quickly poured into a forming box, with an in-mold cooling time of 8 seconds and a foaming time of 1 minute. Ripen for 2 hours, and cut into the required size after 24 hours. The density and tear strength of the polyurethane sponge obtained in each embodiment were tested respectively (refer to GB10808-89). The test results are shown in Table 1.
[0065] Table 1 Performance test results
[0066] .
[0067] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A reinforced and toughened polymer polyol, comprising a base polyether component and a styrene-acrylonitrile copolymer component, characterized in that: The polyether molecular chain of the basic polyether component is connected with a side chain having an ester bond and / or a benzene ring; the molecular chain of the styrene-acrylonitrile copolymer is connected with a side chain having an ester bond and a benzene ring or a side chain having an ester bond and a tertiary amine group. The synthesis process steps are as follows: 1) Adding a polyol initiator, a composite epoxy compound and a catalyst into a reaction kettle, heating the reaction kettle to 40°C to 60°C and reacting the reaction kettle for 5h to 12h to prepare a basic polyether polyol, wherein the composite epoxy compound contains at least one epoxy compound containing an ester bond or an epoxy compound containing a benzene ring; 2) Add AN, SM, modified monomer, initiator, basic polyether polyol, macromolecular dispersant and chain transfer agent into the reactor, react at 115℃~125℃, control the pressure at 0.1MPa~0.5MPa, and the reaction time is 0.5h~2.0h; 3) Distill the remaining monomers in the crude POP and collect the refined POP; In step 1), the proportion of epoxy compounds containing ester bonds and / or epoxy compounds containing benzene rings in the composite epoxy compound is 5 mol% to 50 mol%, and the balance is propylene oxide; wherein the epoxy compounds containing ester bonds include glycidyl acetate, glycidyl butyrate, glycidyl acrylate, glycidyl neodecanoate or glycidyl palmitate; the epoxy compounds containing benzene rings include 2-phenyl-1,2-propylene oxide or styrene oxide; The modified monomer in step 2) is benzyl acrylate, 2-methylstyrene methacrylate or dimethylaminoethyl methacrylate.
2. A reinforced and toughened polymer polyol according to claim 1, characterized in that: The catalyst in step 1) is a DMC catalyst.
3. A reinforced and toughened polymer polyol according to claim 1, characterized in that: The macromolecular dispersant in step 2) is a copolymer of ethylene oxide and glycidyl acrylate or a copolymer of propylene oxide and glycidyl acrylate, and the chain transfer agent is glycerol, ethylene glycol or trimethylolpropane.
4. The reinforced and toughened polymer polyol according to claim 1, characterized in that: The molar ratio of AN, SM, modified monomer, basic polyether polyol, macromolecular dispersant and chain transfer agent described in step 2) is 30~40ː20~40ː5~10ː1ː30~45ː1~10.