A method for synthesizing biodegradable modified PET copolyester material

By adding surface-modified palm fiber and phosphorus-silicon synergistic flame retardants to PET materials, a hydrogen bond association network and a dense carbon layer are formed, which solves the problems of poor flexibility, flammability and insufficient flame retardant properties of PET materials, and achieves The improved mechanical and flame retardant properties of high-performance engineering plastics ensure the safety and environmental protection of the materials.

CN118546505BActive Publication Date: 2024-10-01WUJIANG BODA ELECTRONICS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995165.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Traditional PET materials have safety hazards due to poor molecular chain flexibility, poor impact toughness, flammability and droplet formation when burning, making it difficult to be widely used in the field of high-performance engineering plastics. In addition, existing flame retardants are environmentally polluting and volatile. Migration problem makes it difficult to ensure long-term flame retardant performance.

Method used

Using the synthesis method of biodegradable modified PET copolyester material, palm fiber surface-modified with polyester polyol and a synergistic flame retardant functional agent containing phosphorus and silicon are added to PET to form hydrogen bond association. The network and dense carbon layer improve the mechanical properties and flame retardant properties of the material.

Benefits of technology

It significantly improves the mechanical strength, impact toughness and flame retardant properties of the material, ensuring the application requirements of high-performance engineering plastics, while avoiding environmental pollution and volatile migration of flame retardants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546505B_ABST
    Figure CN118546505B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of materials, and discloses a method for synthesizing a biodegradable modified PET copolyester material. The material is prepared by mixing and melt extruding PET as a base material and auxiliary materials such as a flame retardant functional agent, a plant fiber additive, and a volume extender. The flame retardant functional agent can produce a conjugated effect with a benzene ring in a PET molecular chain in a subsequent high-temperature melt extrusion process, and active hydroxyl groups can produce hydrogen bond associations with PET, so that the flame retardant functional agent can produce a strong interaction with the PET matrix, making it difficult for the flame retardant functional agent to migrate and volatilize, thereby improving the flame retardant performance of the material. The plant fiber additive can play a good stress load transfer effect and enhance the mechanical strength of the material. On the other hand, the flexible structure of polyester polyol is utilized to improve the flexibility of the PET molecular chain and the impact toughness of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a method for synthesizing a biodegradable modified PET copolyester material. Background Art

[0002] As environmental problems become increasingly severe, traditional plastic materials are controversial due to their difficult-to-degrade properties. In this context, the development of new environmentally friendly materials has become a common goal of scientific research and industry. Among them, polyethylene terephthalate (PET) has become one of the substitutes for traditional petroleum-based non-degradable plastics with its unique biodegradable advantages. Since PET contains a large number of rigid benzene ring structures, it has good wear resistance, heat resistance and chemical resistance. It has been widely used in fabrics, packaging materials, engineering plastics and other fields, and its usage has increased year by year. It has become the second largest synthetic polymer material after polyolefins.

[0003] It is precisely because PET contains a large number of rigid benzene rings in its structure, which can bring it more advantages, but it also leads to poor flexibility of its molecular chain and poor impact toughness. In addition, as a polymer material, it is a flammable material, and it will produce molten droplets when burning, causing the fire to spread, posing a major safety hazard. These shortcomings have largely caused huge obstacles to the application of PET in the field of high-performance engineering plastics. Therefore, it is urgent to develop PET materials with better comprehensive performance.

[0004] The invention patent with application number CN202010589386.X discloses a flame-retardant PET material and a preparation method thereof. By adding decabromodiphenyl ether and modified zinc borate to form a composite flame retardant, the flame retardant and mechanical properties of the PET material are improved. However, halogen flame retardants produce a large amount of harmful gases during combustion, which is not conducive to environmental protection, so they are gradually eliminated, and most non-halogen phosphorus flame retardants are prone to volatile migration, so it is difficult to ensure the long-term flame retardant performance of PET. Based on this, the present invention provides a biodegradable modified PET copolyester material with good mechanical properties and excellent flame retardant properties, which can meet the requirements of high-performance engineering plastics. Summary of the invention

[0005] In view of the deficiencies of the prior art, the present invention provides a method for synthesizing a biodegradable modified PET copolyester material.

[0006] A method for synthesizing a biodegradable modified PET copolyester material, wherein the modified PET copolyester material comprises the following raw materials in parts by weight: 65-75 parts of PET, 2-6 parts of a flame retardant functional agent, 1-3.5 parts of a plant fiber additive, 10-15 parts of a compatibilizer, 0.5-1.5 parts of an antioxidant, and 1-2 parts of a lubricant;

[0007] The synthesis method comprises the following steps:

[0008] S1. Prepare all raw materials according to weight;

[0009] S2, adding PET, flame retardant functional agent, plant fiber additive, bulking agent, antioxidant and lubricant into a mixer, stirring and mixing mechanically, feeding into a twin-screw extruder through a feeding hopper, setting the temperature of each zone to 270±5℃, 280±5℃, 285±5℃, 285±5℃, 280±5℃, 275±5℃, the head temperature to 270±5℃, the screw speed to 200-300rpm, forming masterbatch through melt extrusion, and pelletizing to obtain a modified PET copolyester material;

[0010] The plant fiber additive is palm fiber with polyester polyol modified on the surface.

[0011] Furthermore, the preparation method of the flame retardant functional agent is as follows:

[0012] Add 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane and N,N-dimethylformamide to a reactor filled with nitrogen, start stirring, mix well, then add the reactive phosphorus-containing reagent to the reactor, introduce nitrogen protection, gradually heat up to 100-110°C, continue stirring for 3-6 hours, then remove nitrogen, evaporate to remove solvent, cool and discharge, collect solid matter, and then obtain a flame retardant functional agent.

[0013] Furthermore, the reactive phosphorus-containing reagent is diethyl phosphite or dimethyl phosphite.

[0014] Furthermore, the molar ratio of the 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane to the reactive phosphorus-containing reagent is 1:2.

[0015] Specifically, 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane contains two equivalents of epoxy substituents in its structure, which can undergo a ring-opening reaction with the PH in the structure of phosphite-type reactive phosphorus-containing reagents under high temperature conditions to form a synergistic flame retardant containing both silicon and phosphorus flame retardant elements in its structure, i.e., a flame retardant functional agent.

[0016] Furthermore, the preparation method of the plant fiber additive comprises the following steps:

[0017] SS1. Disperse palm fiber in tetrahydrofuran to form a dispersion, then add chloroethyl isocyanate to the dispersion, turn on the heating, gradually increase the temperature to 60-70°C, and add a metal tin catalyst. After the addition, continue stirring for 3-5 hours, discharge the material, separate and collect the fiber material, and obtain a palm fiber modified product;

[0018] SS2. Mix the modified palm fiber with toluene solvent, disperse it by ultrasonic until a homogeneous dispersion is formed, then add sodium hydroxide aqueous solution to the dispersion, stir it at 50-60°C for 2-4h, then add polyether polyol, and after the addition, gradually heat it to 70-80°C, maintain it at this temperature for 4-6h, cool it down and discharge it to obtain a plant fiber additive.

[0019] Furthermore, in step SS1, the length of the palm fiber is 1-3 mm.

[0020] Furthermore, in step SS1, the metal tin catalyst is any one of dibutyltin didodecylsulfide, stannous octoate or dibutyltin dilaurate.

[0021] Furthermore, in step SS2, the mass fraction of the sodium hydroxide aqueous solution is 20-30%.

[0022] Furthermore, in the step SS2, the polyether polyol is a polyether diol or a polyether triol.

[0023] Specifically, by using a metal tin catalyst, the hydroxyl groups on the surface of the palm fiber are catalyzed to react with the isocyanate groups in the structure of chloroethyl isocyanate to undergo an amine esterification reaction, thereby modifying the surface of the palm fiber with halogen substituents to obtain a palm fiber modified product. Then, by using sodium hydroxide for catalysis, the halogen groups can be further replaced with the hydroxyl groups in the structure of the polyether polyol, thereby grafting a macromolecular polyether polyol on the surface of the palm fiber to obtain a fiber additive.

[0024] Furthermore, the compatibilizer is maleic anhydride grafted polyethylene or maleic anhydride grafted polypropylene; the antioxidant is any one of antioxidant 1076, antioxidant 168 or antioxidant 1010; and the lubricant is any one of polyethylene wax, zinc stearate, calcium stearate or stearic acid.

[0025] The beneficial technical effects are:

[0026] (1) The flame retardant functional agent prepared by the present invention contains a rigid benzene ring and an active hydroxyl group generated by a ring-opening reaction. In the subsequent high-temperature melt extrusion process, the rigid benzene ring can produce a conjugated effect with the benzene ring in the PET molecular chain, and the active hydroxyl group can produce a hydrogen bond with PET, so that the flame retardant functional agent can produce a strong interaction with the PET matrix, making it difficult for it to migrate and volatilize. In addition, the flame retardant functional agent structure also contains flame retardant elements phosphorus and silicon. When the material burns, it can quickly form a dense carbon layer of deposited silicon oxide to prevent further combustion of the material, thereby improving the flame retardant performance of the material.

[0027] (2) The present invention prepares palm fiber with a surface modified with a macromolecule as polyester polyol as a plant fiber additive. First, the polyester polyol structure ends contain hydroxyl groups, which can also form hydrogen bonds with PET molecular chains, thereby forming an interwoven structure with palm fiber as the center of the hydrogen bond network. On the one hand, the advantages of palm fiber are utilized to achieve a good stress load transfer effect and enhance the mechanical strength of the material. On the other hand, the flexible structure of polyester polyol is utilized to improve the flexibility of the PET molecular chain and the impact toughness of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0029] Figure 1 This is a schematic diagram of the preparation principle of the flame retardant functional agent;

[0030] Figure 2 It is the infrared spectrum of the flame retardant functional agent;

[0031] Figure 3 This is a schematic diagram of the preparation of plant fiber additives;

[0032] Figure 4 The scanning electron microscope images of palm fiber and plant fiber additives, wherein (A) is palm fiber and (B) is plant fiber additive;

[0033] Figure 5 This is the infrared spectrum of plant fiber additives. DETAILED DESCRIPTION

[0034] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Example 1

[0035] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 65 parts of PET, 2 parts of flame retardant functional agent, 1 part of plant fiber additive, 10 parts of maleic anhydride grafted polyethylene as a compatibilizer, 0.5 parts of antioxidant 1076, and 1 part of lubricant polyethylene wax;

[0036] The preparation method of the modified PET copolyester material comprises the following steps:

[0037] S1. Prepare all raw materials according to weight;

[0038] S2. Add PET, flame retardant functional agent, plant fiber additive, compatibilizer maleic anhydride grafted polyethylene, antioxidant 1076 and lubricant polyethylene wax into a mixer, stir mechanically to mix, feed into a twin-screw extruder through a feeding hopper, set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280°C, and 275°C in sequence, set the head temperature to 270°C, and the screw speed to 200rpm. Form masterbatch through melt extrusion, and cut into pellets to obtain modified PET copolyester material. Example 2

[0039] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 70 parts of PET, 5 parts of flame retardant functional agent, 3 parts of plant fiber additive, 12 parts of maleic anhydride grafted polypropylene as a compatibilizer, 1 part of antioxidant 168, and 1.5 parts of lubricant zinc stearate;

[0040] The preparation method of the modified PET copolyester material comprises the following steps:

[0041] S1. Prepare all raw materials according to weight;

[0042] S2. Add PET, flame retardant functional agent, plant fiber additive, maleic anhydride grafted polypropylene (VAP) compatibilizer, antioxidant 168 and zinc stearate (LAP) lubricant into a mixer, stir and mix them mechanically, and feed them into a twin-screw extruder through a feeding hopper. Set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280±5°C and 275°C, respectively. Set the head temperature to 270°C and the screw speed to 280rpm. Form masterbatch through melt extrusion and pelletize to obtain modified PET copolyester material. Example 3

[0043] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 75 parts of PET, 6 parts of flame retardant functional agent, 3.5 parts of plant fiber additive, 15 parts of maleic anhydride grafted polypropylene as a compatibilizer, 1.5 parts of antioxidant 1010, and 2 parts of lubricant calcium stearate;

[0044] The preparation method of the modified PET copolyester material comprises the following steps:

[0045] S1. Prepare all raw materials according to weight.

[0046] S2. Add PET, flame retardant functional agent, plant fiber additive, compatibilizer maleic anhydride grafted polypropylene, antioxidant 1010 and lubricant calcium stearate into a mixer, stir and mix mechanically, feed them into a twin-screw extruder through a feeding hopper, set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280°C, and 275°C in sequence, set the head temperature to 270°C, and the screw speed to 300rpm. Form masterbatch through melt extrusion, and cut into pellets to obtain modified PET copolyester material.

[0047] Comparative Example 1

[0048] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 70 parts of PET, 5 parts of diethyl phosphite, 3 parts of plant fiber additive, 12 parts of maleic anhydride grafted polypropylene as a compatibilizer, 1 part of antioxidant 168, and 1.5 parts of zinc stearate as a lubricant;

[0049] The preparation method of the modified PET copolyester material comprises the following steps:

[0050] S1. Prepare all raw materials according to weight.

[0051] S2. Add PET, diethyl phosphite, plant fiber additive, maleic anhydride grafted polypropylene as a compatibilizer, antioxidant 168 and zinc stearate as a lubricant into a mixer, stir and mix them mechanically, and feed them into a twin-screw extruder through a feeding hopper. Set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280±5°C, and 275°C, respectively. Set the head temperature to 270°C and the screw speed to 280rpm. Form masterbatch through melt extrusion and pelletize to obtain modified PET copolyester material.

[0052] Comparative Example 2

[0053] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 70 parts of PET, 3 parts of plant fiber additives, 12 parts of maleic anhydride grafted polypropylene as a compatibilizer, 1 part of antioxidant 168, and 1.5 parts of lubricant zinc stearate;

[0054] The preparation method of the modified PET copolyester material comprises the following steps:

[0055] S1. Prepare all raw materials according to weight;

[0056] S2. Add PET, plant fiber additives, maleic anhydride grafted polypropylene (PP) as a compatibilizer, antioxidant 168 and zinc stearate as a lubricant into a mixer. After mechanical stirring and mixing, feed them into a twin-screw extruder through a feeding hopper. Set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280±5°C and 275°C, respectively. Set the head temperature to 270°C and the screw speed to 280rpm. Form masterbatch through melt extrusion and pelletize to obtain modified PET copolyester material.

[0057] Comparative Example 3

[0058] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 70 parts of PET, 5 parts of flame retardant functional agent, 3 parts of palm fiber, 12 parts of maleic anhydride grafted polypropylene as a compatibilizer, 1 part of antioxidant 168, and 1.5 parts of zinc stearate as a lubricant;

[0059] The preparation method of the modified PET copolyester material comprises the following steps:

[0060] S1. Prepare all raw materials according to weight;

[0061] S2. Add PET, flame retardant functional agent, palm fiber, compatibilizer maleic anhydride grafted polypropylene, antioxidant 168 and lubricant zinc stearate into a mixer, stir and mix mechanically, feed them into a twin-screw extruder through a feeding hopper, set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280±5°C, and 275°C, set the head temperature to 270°C, and the screw speed to 280rpm. Form masterbatch through melt extrusion, and cut into pellets to obtain modified PET copolyester material.

[0062] Comparative Example 4

[0063] A biodegradable modified PET copolyester material comprises the following raw materials in parts by weight: 70 parts of PET, 5 parts of flame retardant functional agent, 12 parts of maleic anhydride grafted polypropylene as a compatibilizer, 1 part of antioxidant 168, and 1.5 parts of lubricant zinc stearate;

[0064] The preparation method of the modified PET copolyester material comprises the following steps:

[0065] S1. Prepare all raw materials according to weight;

[0066] S2. Add PET, flame retardant functional agent, compatibilizer maleic anhydride grafted polypropylene, antioxidant 168 and lubricant zinc stearate into a mixer, stir and mix mechanically, feed them into a twin-screw extruder through a feeding hopper, set the temperatures of each zone to 270°C, 280°C, 285°C, 285°C, 280±5°C, and 275°C, set the head temperature to 270°C, and the screw speed to 280rpm. Form masterbatch through melt extrusion, and cut into pellets to obtain modified PET copolyester material.

[0067] The flame retardant functional agent used in the above examples and comparative examples was prepared by the following method:

[0068] Add 0.6 g of 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane and N,N-dimethylformamide to a reactor filled with nitrogen, start stirring, mix well, then add 0.33 g of diethyl phosphite to the reactor, pass nitrogen for protection, gradually heat to 110°C, continue stirring for 4 hours, then remove nitrogen, evaporate to remove solvent, cool and discharge, collect solids, and a flame retardant functional agent can be obtained.

[0069] The CAS number of 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane is 865811-59-2, which was purchased from Shanghai Myrel Biochemical Technology Co., Ltd., and the CAS number of diethyl phosphite is 762-04-9, which was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0070] The preparation principle of the flame retardant functional agent is as follows Figure 1 shown.

[0071] The flame retardant functional agent was made into a potassium bromide tablet test sample and infrared test was performed. The results are as follows Figure 2 As shown, 3292cm -1 The absorption peak at 3000-3100 cm is the characteristic absorption peak of hydroxyl group produced by the ring-opening reaction of 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane and diethyl phosphite. -1 The absorption peak at 1230 cm is the characteristic absorption peak of CH in the benzene ring. -1 The absorption peak at 1101cm is the characteristic absorption peak of P=O. -1 The absorption peak that appears at is the Si-O characteristic absorption peak.

[0072] The plant fiber additives used in the above examples and comparative examples are prepared by the following method:

[0073] SS1. Disperse 12 g of palm fiber with a length of 2 mm in tetrahydrofuran to form a dispersion, then add 5.5 g of chloroethyl isocyanate to the dispersion, turn on the heating, gradually increase the temperature to 65°C, and add 0.2 g of dibutyltin dilaurate. After the addition, continue stirring for 4 hours, discharge the material, separate and collect the fiber material, and obtain a palm fiber modified product;

[0074] SS2. Mix 6.5 g of palm fiber modification with toluene solvent, disperse by ultrasonic until a homogeneous dispersion is formed, then add 20 mL of 30% sodium hydroxide aqueous solution to the dispersion, stir at 55 °C for 3 h, and then add 15 g of polyether polyol. After the addition, gradually heat to 75 °C, maintain at this temperature for 5 h, cool and discharge to obtain a plant fiber additive.

[0075] The CAS number of chloroethyl isocyanate is 1943-83-5, which was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. The CAS number of polyether polyol is 9003-11-6, which was purchased from Tianjin Xiensi Biochemical Technology Co., Ltd., with a brand number of P-90132.

[0076] The preparation principle of the plant fiber additive is as follows Figure 3 shown.

[0077] Figure 4 These are scanning electron microscope images of palm fiber and plant fiber additives, where (A) is palm fiber and (B) is plant fiber additive. It can be clearly seen that the surface of palm fiber is relatively smooth without obvious special marks, while the surface of plant fiber additive clearly shows a special concave-convex morphology with obvious modification marks.

[0078] Figure 5 This is the infrared analysis test chart of the plant fiber additive, where 3389cm -1 The absorption peak at 3185 cm is the characteristic absorption peak of NH in the amine ester bond. -1 The absorption peak at 2800-3000cm is the characteristic absorption peak of hydroxyl. -1 The absorption peak at 1715 cm is the characteristic absorption peak of CH in methyl, methylene and methine. -1 The absorption peak at 1142 cm is the characteristic absorption peak of C=O of amine ester bond. -1 The absorption peak that appears at is the CO characteristic absorption peak of the ether bond.

[0079] Test Case

[0080] The materials in Examples 1 to 3 and Comparative Examples 1 to 4 were injection molded into test specimens, and various performance tests were performed. The results are recorded in Table 1:

[0081] Table 1 - Performance test results

[0082]

[0083] The tensile strength is tested according to the standard GB / T 1040-2008; the impact strength is tested according to the standard GB / T 1843-2008; the limiting oxygen index is tested according to the standard GB / T 2406-2008 after the specimens are placed at room temperature for 3 months.

[0084] Analysis of the test data shows that the PET copolyester material prepared by adding flame retardant functional agents and plant fiber additives has significantly better mechanical strength, better impact toughness, and a limiting oxygen index greater than 27%, which is a flame retardant material. After the flame retardant functional agent was replaced with conventional diethyl phosphite to prepare the PET copolyester material, after being placed for 3 months, obvious volatilization migration occurred, causing the flame retardant properties of the material to drop sharply. After the plant fiber additive was replaced with conventional unmodified palm fiber, the mechanical properties and impact toughness were significantly reduced. This is due to the interface problems between the palm fiber and the PET substrate, which makes it difficult to efficiently exert its own advantages in transferring stress loads.

[0085] Based on the ideal embodiment of the present invention, through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.

Claims

1. A method for synthesizing a biodegradable modified PET copolyester material, characterized in that: The modified PET copolyester material comprises the following raw materials in parts by weight: 65-75 parts of PET, 2-6 parts of flame retardant functional agent, 1-3.5 parts of plant fiber additive, 10-15 parts of compatibilizer, 0.5-1.5 parts of antioxidant, and 1-2 parts of lubricant; The preparation method of the flame retardant functional agent is as follows: Add 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane and N,N-dimethylformamide to a reactor filled with nitrogen, start stirring, mix well, then add the reactive phosphorus-containing reagent to the reactor, introduce nitrogen protection, gradually heat up to 100-110°C, continue stirring for 3-6 hours, then remove nitrogen, evaporate to remove solvent, cool and discharge, collect solids, and obtain a flame retardant functional agent; The synthesis method comprises the following steps: S1. Prepare all raw materials according to weight; S2, adding PET, flame retardant functional agent, plant fiber additive, bulking agent, antioxidant and lubricant into a mixer, stirring and mixing mechanically, feeding into a twin-screw extruder through a feeding hopper, setting the temperature of each zone to 270±5℃, 280±5℃, 285±5℃, 285±5℃, 280±5℃, 275±5℃, the head temperature to 270±5℃, the screw speed to 200-300rpm, forming masterbatch through melt extrusion, and pelletizing to obtain a modified PET copolyester material; The preparation method of the plant fiber additive comprises the following steps: SS1. Disperse palm fiber in tetrahydrofuran to form a dispersion, then add chloroethyl isocyanate to the dispersion, turn on the heating, gradually increase the temperature to 60-70°C, and add a metal tin catalyst. After the addition, continue stirring for 3-5 hours, discharge the material, separate and collect the fiber material, and obtain a palm fiber modified product; SS2. Mix the modified palm fiber with toluene solvent, disperse it by ultrasonic until a homogeneous dispersion is formed, then add sodium hydroxide aqueous solution to the dispersion, stir it at 50-60°C for 2-4h, then add polyether polyol, and after the addition, gradually heat it to 70-80°C, maintain it at this temperature for 4-6h, cool it down and discharge it to obtain a plant fiber additive.

2. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: The reactive phosphorus-containing reagent is diethyl phosphite or dimethyl phosphite.

3. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: The molar ratio of the 1,5-bis(glycidoxypropyl)-3-phenyl-1,1,3,5,5-pentamethyltrisiloxane to the reactive phosphorus-containing reagent is 1:

2.

4. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: In the step SS1, the length of the palm fiber is 1-3 mm.

5. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: In the step SS1, the metal tin catalyst is any one of dibutyltin didodecylsulfide, stannous octoate or dibutyltin dilaurate.

6. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: In the step SS2, the mass fraction of the sodium hydroxide aqueous solution is 20-30%.

7. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: In the step SS2, the polyether polyol is a polyether diol or a polyether triol.

8. The method for synthesizing the biodegradable modified PET copolyester material according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polyethylene or maleic anhydride grafted polypropylene; the antioxidant is any one of antioxidant 1076, antioxidant 168 or antioxidant 1010; the lubricant is any one of polyethylene wax, zinc stearate, calcium stearate or stearic acid.