Hot melt adhesive film for single battery and preparation method thereof
By using hot melt adhesive films prepared by using polyolefin resin and other materials in fuel cells, the problems of seal failure, stress concentration and low power density in fuel cell stack sealing technology are solved, and high bond strength and durability are achieved. Simplifies the production process and reduces costs.
Patent Information
- Application Number
- CN202411055544.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing fuel cell stack sealing technology has problems such as the risk of seal failure, the damage to the plate caused by concentrated stress, low power density and easy plastic deformation of the sealing ring.
A hot melt adhesive film consisting of polyolefin resin, polybutadiene resin, tackifying resin, thermoplastic elastomer resin, curing agent and latent curing agent is used, including release layer, hot melt layer and reinforcement layer, and is coated through a scraper. A hot melt adhesive film for single cells with a double-sided hot melt layer is used for sealing the electrode plate and the film electrode.
It improves the sealing performance and service life of fuel cell single cells, reduces production costs, simplifies the production process, avoids glue spills, and maintains sealing and durability at high temperatures.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a hot melt adhesive film for a single cell and a preparation method thereof. Background Art
[0002] A fuel cell is a power generation device that converts the chemical energy present in fuel and oxidant directly into electrical energy. Fuel cells have the advantages of zero emission, no vibration or noise, good load responsiveness, and high reliability. Fuel cells can generally be divided into alkaline fuel cells, phosphoric acid fuel cells, molten carbonate fuel cells, solid oxide fuel cells, and proton exchange membrane fuel cells. Among them, proton exchange membrane fuel cells have high energy conversion efficiency, can be quickly started at room temperature, have no electrolyzed water loss, and have a long life. They have developed rapidly in recent years and are receiving increasing attention.
[0003] Fuel cells usually include a membrane electrode (also called MEA) and a current collector; the membrane electrode of a fuel cell is the electrochemical reaction site where the reducing agent undergoes oxidation reaction and the oxidant undergoes reduction reaction. The traditional membrane electrode mainly includes a proton exchange membrane located in the middle and a cathode and an anode are integrally provided on both sides thereof, and a gas diffusion layer located on the upper and lower surfaces of the proton exchange membrane. In order to promote the occurrence of electrochemical reactions, a catalyst is generally provided between the cathode, the anode and the proton exchange membrane (usually located at the interface between the proton exchange membrane and the gas diffusion layer); and the current collector is usually called a bipolar plate, which is responsible for distributing fuel and air to the surfaces of the positive and negative electrodes and the heat dissipation of the stack. It is also responsible for connecting single cells in series to form a fuel cell stack. It mainly plays the role of separating the oxidant, the reducing agent and the coolant and collecting current. In actual manufacturing, the fluid transmission channels in the fuel cell stack and the fluid transmission channels and the outside of the stack need to be sealed. The leakage of fluids or the mixing of different fluids in the stack not only causes waste and reduces the performance of the stack, but also may cause safety accidents. Therefore, the sealing technology in fuel cell stack technology has a huge impact on the safety, life, efficiency and other aspects of the stack. In the prior art fuel cell stack, an embedding groove is usually set at the edge of the graphite or metal plate that needs to be sealed, and a sealing gasket is placed in the embedding groove, or a circle of glue is applied at the edge of the seal by a glue machine, and then cured and pressed to achieve sealing. However, these sealing methods usually face the following problems:
[0004] a. Generally there is only a single seal to prevent leakage, and the risk of seal failure is high.
[0005] b. A great deal of pressure needs to be applied to the sealing ring to form a good seal, which results in a large stress in a local area of the plate, which can easily lead to damage or distortion of the plate.
[0006] c. It is necessary to preset grooves on the electrode plate, which increases the thickness requirement of the electrode plate and reduces the power density of the fuel cell stack.
[0007] d. A single sealing ring or sealing rubber line is prone to plastic deformation, and the risk of sealing failure is high.
[0008] Therefore, it is very necessary to seek new sealing technology solutions to effectively improve the sealing performance of fuel cell cells. Summary of the invention
[0009] The first technical problem to be solved by the present invention is: in view of the deficiencies in the prior art, a hot melt adhesive film for a single cell is provided, which has good sealing effect and high bonding strength.
[0010] To solve the above-mentioned first technical problem, the technical solution of the present invention is:
[0011] A hot melt adhesive film for a single cell, comprising a release layer, a hot melt layer I, a reinforcement layer and a hot melt layer II arranged in sequence;
[0012] The hot melt layer I and the hot melt layer II are both composed of polyolefin resin, polybutadiene resin, tackifying resin, thermoplastic elastomer resin, curing agent, latent curing agent, and diluting solvent;
[0013] The polyolefin resin is a non-chlorinated acid anhydride-modified polyolefin resin.
[0014] Preferably, the release layer is a PET film coated with a non-silicone resin material on both sides, the coating thickness of the non-silicone resin material is 0.1-0.5 μm, and the thickness of the release layer is 25-150 μm.
[0015] Preferably, the reinforcement layer is made of polypropylene resin material, and the thickness of the reinforcement layer is 16-50 μm.
[0016] Preferably, the weight ratio of the polyolefin resin, the polybutadiene resin, the tackifying resin, the thermoplastic elastomer resin, the curing agent, the latent curing agent and the dilution solvent is 100: (10-30): (10-30): (10-30): (10-30): (1-5): (0.5-2): (50-150).
[0017] The weight average molecular weight of the polyolefin resin is 10,000 to 50,000, and the acid value of the polyolefin resin is 2 to 50 mgKOH / g.
[0018] The polybutadiene resin is a polybutadiene resin modified with a hydroxyl group, a carboxyl group or an epoxy group. The epoxy-modified polybutadiene resin is obtained by an oxidation reaction between a low molecular weight liquid polybutadiene resin and a peroxide diacid, and the reaction principle is as follows:
[0019]
[0020] The tackifying resin is one of petroleum resin, terpene resin and terpene phenolic resin;
[0021] The thermoplastic elastomer resin is an amino-terminated SEBS material.
[0022] The curing agent is one of an epoxy curing agent, a non-blocked isocyanate curing agent, and a carbodiimide curing agent;
[0023] The latent curing agent is a blocked isocyanate curing agent, and the deblocking temperature of the blocked isocyanate curing agent is 110-130°C.
[0024] The thickness of the hot-melt layer I and the hot-melt layer II are both 20-45 μm.
[0025] The dilution solvent is any one of ethyl acetate, acetone, butanone, cyclohexanone, methyl isobutyl ketone, toluene, xylene, and cyclohexane, or a mixed solution of two or more thereof.
[0026] The second technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for preparing a hot melt adhesive film for a single cell is provided, and the prepared hot melt adhesive film for a single cell has good sealing effect and high bonding strength.
[0027] To solve the above second technical problem, the technical solution of the present invention is:
[0028] A method for preparing a hot melt adhesive film for a single cell comprises the following steps:
[0029] S01. Preparation of polyolefin resin
[0030] Add polyolefin, toluene, acid anhydride and di-tert-butyl peroxide into an autoclave, heat while stirring, and react at 140-160° C. for 1-3 hours to obtain a reaction liquid, wherein the weight ratio of polyolefin, toluene, acid anhydride and di-tert-butyl peroxide is 100: (400-600): (15-25): (3-5);
[0031] The reaction solution is cooled to 40° C. to obtain a non-chlorinated acid anhydride-modified polyolefin resin;
[0032] S02. Preparation of hot melt adhesive
[0033] Adding polybutadiene resin, tackifying resin and thermoplastic elastomer resin to the non-chlorinated anhydride modified polyolefin resin solution prepared in S01, cooling to room temperature after complete dissolution and filtering, adding curing agent, latent curing agent and diluent solvent to the filtrate, stirring evenly and filtering through a 200-800 mesh filter or a 1-20 μm filter element to obtain a hot melt layer adhesive;
[0034] S03. Preparation of hot melt adhesive film for single cell
[0035] A hot melt adhesive layer is coated on one side of the reinforcing layer using a blade coater or a CED coater, and a release layer is attached after drying to obtain a hot melt adhesive film with a single-sided hot melt layer;
[0036] The other side of the reinforcement layer is coated with a hot melt layer adhesive by a blade coater or a CED coater, and after aging, a hot melt adhesive film for a single cell with a double-sided hot melt layer is obtained.
[0037] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0038] 1. The present invention adopts a hot melt adhesive film product with hot melt bonding effect, which is used for bonding and sealing the single cell plate of the fuel cell with the packaged membrane electrode, and no longer needs to be sealed by dispensing or injection molding, so that the single cell manufacturing process is simple and the efficiency and yield are significantly improved.
[0039] 2. The present invention uses materials without N, P, S and Al, Cu, Ni, Cd, Cr, Pb, and Fe to make the hot melt layer, thereby avoiding the precipitation problem of the hot melt adhesive film after long-term acid immersion, thereby greatly improving the service life of the single battery.
[0040] 3. The present invention greatly improves the durability of the hot melt adhesive film by selecting polypropylene resin with excellent physical and mechanical properties, gas barrier properties, chemical stability, and hydrolysis resistance, acid resistance, alkali resistance, heat resistance, UV resistance, radiation resistance and other properties as the reinforcement layer; and matches the hot melt layer material with high bonding strength and low precipitates as well as extremely low water vapor, hydrogen and oxygen permeability to ensure that the hot melt adhesive film has excellent aging resistance, low precipitation and sealing, thereby improving the service life of the fuel cell stack.
[0041] 4. The present invention uses polypropylene resin as a reinforcement layer, which can not only improve the stiffness of the hot melt adhesive film and facilitate product die-cutting processing, but also has high adhesion with the polyolefin resin material of the hot melt layer to avoid stratification and debonding. At the same time, the use of the polypropylene resin reinforcement layer can reduce the amount of hot melt layer glue used, reducing the production cost of the hot melt adhesive film. Moreover, this hot melt adhesive film can greatly improve the efficiency and yield in the single cell packaging process, which is beneficial to the industrialization of single cell products.
[0042] 5. The present invention mixes conventional curing agents and closed curing agents to ensure that the hot melt adhesive film has high bonding strength and sealing properties in the early stage of single cell production without glue overflow problems. During use, the closed curing agent further reacts and cross-links due to high temperature, thereby avoiding the problem of insufficient sealing due to long-term compression and thinning of the glue overflow thickness under high temperature conditions, and also reduces the degree of attenuation of peel strength. DETAILED DESCRIPTION
[0043] The present invention will be further described below in conjunction with the embodiments. Example 1
[0044] 1. Add 100g of propylene-ethylene copolymer (melting point 85°C), 400g of toluene, 15g of maleic anhydride, and 3g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 140°C for 3h. After cooling the obtained reaction solution to 40°C, 510g of non-chlorinated anhydride-modified polyolefin resin (acid value 12mgKOH / g, weight average molecular weight 45000, melting point 84°C) is obtained;
[0045] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 10g of Japan Tosoh epoxidized polybutadiene resin PB3600, 10g of Arizona terpene resin RE100L and 10g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0046] 3. Add 1g of Japanese polyurethane isocyanate curing agent L-75, 1g of Lanxess blocked isocyanate curing agent BI7982 and 50g of toluene dilution solvent to the filtered hot melt adhesive solution, stir evenly, and filter with a 400-mesh filter. Then use a scraper coater to coat a 22μm hot melt adhesive layer on one side of the 16μm polypropylene resin reinforcement layer. After drying completely, attach a 38um release layer and roll it up. Use the same method to prepare the hot melt layer on the other side. After aging, a single cell hot melt adhesive film with a double-sided hot melt layer is obtained. Example 2
[0047] 1. Add 100g of propylene-ethylene-1-butene copolymer (melting point 95°C), 500g of toluene, 20g of maleic anhydride, and 4g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 150°C for 2h. After cooling the obtained reaction solution to 40°C, 620g of non-chlorinated anhydride-modified polyolefin resin (acid value 19mgKOH / g, weight average molecular weight 48000, melting point 93°C) is obtained;
[0048] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 15g of Japan Tosoh epoxidized polybutadiene resin PB3600, 15g of Arizona terpene resin RE100L and 15g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0049] 3. Add 1.5g of Japanese polyurethane isocyanate curing agent L-75, 2g of Lanxess blocked isocyanate curing agent BI7982 and 100g of cyclohexane dilution solvent to the filtered hot melt adhesive solution, stir evenly and filter with a 400-mesh filter. Then use a scraper coater to apply a 22μm hot melt adhesive layer on one side of the 16μm polypropylene resin reinforcement layer. After drying completely, attach a 25um release layer and roll it up. Use the same method to prepare the hot melt layer on the other side. After aging, a single cell hot melt adhesive film with double-sided hot melt layers is obtained. Example 3
[0050] 1. Add 100g of propylene-ethylene copolymer (melting point 85°C), 400g of toluene, 15g of maleic anhydride, and 3g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 150°C for 2h. After cooling the obtained reaction solution to 40°C, 505g of non-chlorinated anhydride-modified polyolefin resin (acid value 12mgKOH / g, weight average molecular weight 45000, melting point 84°C) is obtained;
[0051] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 20g of Japan Tosoh epoxidized polybutadiene resin PB3600, 10g of Arizona terpene resin NG98 and 13g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0052] 3. Add 1.2g of Japanese polyurethane isocyanate curing agent L-75, 1g of Covestro blocked isocyanate curing agent BL3175 and 85g of butanone diluent solvent to the filtered hot melt adhesive solution, stir evenly, and filter with a 400-mesh filter. Then use a scraper coater to apply a 20μm hot melt adhesive layer on one side of the 25μm polypropylene resin reinforcement layer. After drying completely, attach a 100um release layer and roll it up. Use the same method to prepare the hot melt layer on the other side. After aging, a single cell hot melt adhesive film with a double-sided hot melt layer is obtained. Example 4
[0053] 1. Add 100g of propylene-ethylene copolymer (melting point 85°C), 600g of toluene, 15g of maleic anhydride, and 3g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 160°C for 1h. After cooling the obtained reaction solution to 40°C, 700g of non-chlorinated anhydride-modified polyolefin resin (acid value 12mgKOH / g, weight average molecular weight 45000, melting point 84°C) is obtained;
[0054] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 30g of Japan Tosoh epoxidized polybutadiene resin PB3600, 30g of Arizona terpene resin RE100L and 30g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0055] 3. Add 5g of Starr carbodiimide curing agent XR-5580, 1g of Lanxess blocked isocyanate curing agent BI7982 and 100g of ethyl acetate diluent to the filtered hot melt adhesive solution, stir evenly and filter with a 400-mesh filter. Then use a scraper coater to apply a 25μm hot melt layer on one side of the 50μm polypropylene resin reinforcement layer. After drying, attach a 150um release layer and roll it up. Use the same method to prepare the hot melt layer on the other side. After aging, a single cell hot melt adhesive film with double-sided hot melt layers is obtained. Example 5
[0056] 1. Add 100g of propylene-ethylene-1-butene copolymer (melting point 90°C), 480g of toluene, 25g of maleic anhydride, and 5g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 150°C for 2h. After cooling the obtained reaction solution to 40°C, 600g of non-chlorinated acid anhydride-modified polyolefin resin (acid value 23mgKOH / g, weight average molecular weight 47000, melting point 87°C) is obtained;
[0057] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 15g of Japan Tosoh epoxidized polybutadiene resin PB3600, 20g of Arizona terpene resin RE100L and 15g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0058] 3. Add 3g Nan Ya epoxy resin NPES901, 0.5g Lanxess blocked isocyanate curing agent BI7982 and 150g mixed dilution solvent of cyclohexanone and xylene (the volume ratio of cyclohexanone and xylene is 1:1) to the filtered hot melt adhesive solution, stir evenly and filter with a 400-mesh filter. Then use a scraper coater to apply a 40μm hot melt adhesive layer on one side of the 25μm polypropylene resin reinforcement layer. After drying, attach a 50um release layer and roll it up. Use the same method to prepare the hot melt layer on the other side. After aging, a single cell hot melt adhesive film with double-sided hot melt layers is obtained. Comparative Example 1
[0059] The isocyanate curing agent L-75 of Japanese polyurethane was not added, and the rest was exactly the same as in Example 2. Comparative Example 2
[0060] The LANXESS blocked isocyanate curing agent BI7982 was not added, and the rest was exactly the same as in Example 2.
[0061] The performance of the hot melt adhesive film products for single cells in the above-mentioned Examples 1-5 and Comparative Examples 1-2 were tested respectively. The specific test items and test methods are shown in Table 1 below, and the test results are shown in Table 2.
[0062] Table 1
[0063]
[0064] Table 2
[0065]
[0066] Among them, the peel strength test adopts 140℃*60s*0.6Mpa hot pressing.
[0067] It can be seen from the experimental data in the above table that a hot melt adhesive film material having excellent bonding strength to the electrode plate and the membrane electrode PEN frame and a low drop in peel strength after acid immersion can be obtained by adding different proportions; at the same time, the hot melt adhesive film prepared by the present invention has a small drop in peel strength after long-term immersion in acid and no precipitates affect the activity of the membrane electrode; the present invention uses acid-modified polyolefins, polybutadiene resins with functional groups, and styrene thermoplastic elastomers with terminal amino groups to react and cross-link with a curing agent to form an interpenetrating network structure, ensuring that there is no glue overflow during the initial hot pressing of the product, and the addition of latent curing agents can further cross-link to achieve the purpose of post-stage curing, thereby improving the temperature resistance and hydrolysis resistance of the hot melt adhesive film and reducing compression deformation; the present invention uses OPP material as a reinforcing layer, which can not only improve the stiffness of the hot melt adhesive film and facilitate product die-cutting processing, but also has high adhesion to the polyolefin resin material of the bonding layer to avoid stratification and debonding, and at the same time, the use of a polypropylene reinforcement layer can reduce the amount of hot melt adhesive layer glue used, thereby reducing the production cost of the hot melt adhesive film.
[0068] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
Claims
1. A hot melt adhesive film for a single cell, characterized in that: It includes a release layer, a hot-melt layer I, a reinforcement layer and a hot-melt layer II which are arranged in sequence; The hot melt layer I and the hot melt layer II are both composed of polyolefin resin, polybutadiene resin, tackifying resin, thermoplastic elastomer resin, curing agent, latent curing agent, and diluting solvent; The polyolefin resin is a non-chlorinated anhydride-modified polyolefin resin; The method for preparing the hot melt adhesive film for a single cell comprises the following preparation steps: S01. Preparation of polyolefin resin Add polyolefin, toluene, acid anhydride and di-tert-butyl peroxide into an autoclave, stir and heat, and react at 140-160°C for 1-3 hours to obtain a reaction liquid, wherein the weight ratio of polyolefin, toluene, acid anhydride and di-tert-butyl peroxide is 100: (400-600): (15-25): (3-5); The reaction solution is cooled to 40° C. to obtain a non-chlorinated acid anhydride-modified polyolefin resin; S02. Preparation of hot melt adhesive Adding polybutadiene resin, tackifying resin and thermoplastic elastomer resin to the non-chlorinated anhydride modified polyolefin resin solution prepared in S01, cooling to room temperature after complete dissolution and filtering, adding curing agent, latent curing agent and diluent solvent to the filtrate, stirring evenly and filtering through a 200-800 mesh filter or a 1-20 μm filter element to obtain a hot melt layer adhesive; S03. Preparation of hot melt adhesive film for single cell A hot melt adhesive layer is coated on one side of the reinforcing layer using a blade coater or a CED coater, and a release layer is attached after drying to obtain a hot melt adhesive film with a single-sided hot melt layer; The other side of the reinforcement layer is coated with a hot melt layer adhesive by a blade coater or a CED coater, and after aging, a hot melt adhesive film for a single cell with a double-sided hot melt layer is obtained.
2. A hot melt adhesive film for a single cell as claimed in claim 1, characterized in that: The release layer is a PET film coated with a non-silicone resin material on both sides, the coating thickness of the non-silicone resin material is 0.1-0.5 μm, and the thickness of the release layer is 25-150 μm.
3. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The reinforcement layer is made of polypropylene resin material, and the thickness of the reinforcement layer is 16-50 μm.
4. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The weight ratio of the polyolefin resin, the polybutadiene resin, the tackifying resin, the thermoplastic elastomer resin, the curing agent, the latent curing agent and the dilution solvent is 100: (10-30): (10-30): (10-30): (10-30): (1-5): (0.5-2): (50-150).
5. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The weight average molecular weight of the polyolefin resin is 10,000 to 50,000, and the acid value of the polyolefin resin is 2 to 50 mgKOH / g.
6. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The polybutadiene resin is a polybutadiene resin modified with a hydroxyl group, a carboxyl group or an epoxy group.
7. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The tackifying resin is one of petroleum resin, terpene resin and terpene phenolic resin; The thermoplastic elastomer resin is an amino-terminated SEBS material.
8. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The curing agent is one of an epoxy curing agent, a non-blocked isocyanate curing agent, and a carbodiimide curing agent; The latent curing agent is a blocked isocyanate curing agent, and the deblocking temperature of the blocked isocyanate curing agent is 110-130°C; The thickness of the hot-melt layer I and the hot-melt layer II are both 20-45 μm.
9. The hot melt adhesive film for a single cell according to claim 1, characterized in that: The dilution solvent is any one of ethyl acetate, acetone, butanone, cyclohexanone, methyl isobutyl ketone, toluene, xylene, and cyclohexane, or a mixed solution of two or more thereof.