A high wear-resistant and corrosion-resistant Ni-based coating and preparation method thereof

By doping Hf in NiAl coating and using arc ion plating technology to generate a dense Al2O3 layer, the problems of complex and high cost of NiAl intermetallic compound/ceramic matrix composite materials in the prior art are solved, and high wear resistance is achieved Corrosion-resistant coating improves the hardness and service life of the material.

CN118563258BActive Publication Date: 2024-11-26CHINA CONSTR MACHINERY TEST CENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411056112.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-26
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

In the prior art, when preparing NiAl intermetallic compound/ceramic matrix composites, the process is complex, the energy consumption is large, and the production efficiency is low, resulting in high production costs, weak binding force between the hard phase and the matrix, and cracks and pore defects are prone to occur.

Method used

By doping 0.05 at.% Hf in NiAl coating, the NiAlHf coating is deposited using arc ion plating technology, and a dense Al2O3 layer is generated at high temperature, improving the adhesion and wear resistance of the coating, combined with arc ion plating Fast and low cost characteristics.

Benefits of technology

A Ni-based coating with high wear resistance and corrosion resistance is achieved, providing excellent resistance to high temperature oxidation, enhancing the hardness and wear resistance of the material, extending service life, and avoiding weak bonding and defect problems in traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563258B_ABST
    Figure CN118563258B_ABST
Patent Text Reader

Abstract

The present invention provides a highly wear-resistant and corrosion-resistant Ni-based coating and a preparation method thereof, which belongs to the technical field of material surface. The element composition includes: in atomic percentage, 49.5 at. % Al, 0.05 at. % Hf, and the rest is Ni; the preparation method includes: target material preparation: preparing NiAlHf target material according to the atomic percentage content of Al, Hf and Ni; selecting substrate: selecting a high-temperature alloy substrate, and pre-treating the surface of the high-temperature alloy substrate; depositing NiAlHf coating: placing the high-temperature alloy substrate in a deposition furnace, and using an arc ion plating method to deposit the NiAlHf coating on the surface of the high-temperature alloy substrate, and subjecting the coating to vacuum heat treatment to obtain a highly wear-resistant and corrosion-resistant Ni-based coating. The present invention promotes the generation of continuous, dense, and well-adherent Al on the surface of the coating by doping the NiAl coating with 0.05 at. % Hf. 2 O 3 layer to provide excellent resistance to high temperature oxidation, improve the hardness and wear resistance of the material, give the material good high temperature mechanical properties, and extend its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material surface, in particular to a highly wear-resistant and corrosion-resistant Ni-based coating and a preparation method thereof. Background Art

[0002] Nickel-based high-temperature alloys have become the preferred material for aviation gas turbine blades due to their excellent high-temperature mechanical properties. Turbine blades are subjected to large alternating loads during operation, and the blade tenons that fit closely with the turbine disk are prone to micro-motion wear, inducing micro-motion damage, which in turn leads to turbine blade failure, which has become one of the main reasons for the high incidence of aircraft engine failures. Components used in high-temperature service environments, especially those located in gas turbine processes, not only require oxidation resistance to maintain their corresponding expected performance, but also need to meet the actual requirements of the alloy to resist friction and wear during long-term use.

[0003] NiAl intermetallic compounds are used as high-temperature alloys or coating materials due to their high specific strength and specific stiffness, good thermal conductivity and electrical conductivity, excellent thermal stability and corrosion resistance. Adding ceramic particles into the NiAl intermetallic compound matrix to form a NiAl intermetallic compound composite material reinforced and toughened with ceramic particles can not only strengthen the NiAl intermetallic compound, but also combine the excellent properties of ceramic materials to prepare NiAl intermetallic compound / ceramic matrix composite materials with excellent wear resistance, high temperature resistance and oxidation resistance. At present, the commonly used process methods for preparing NiAl intermetallic compound / ceramic matrix composite materials are mechanical alloying, hot pressing exothermic reaction synthesis, hot pressing sintering and hot pressing reaction synthesis, etc. The preparation process is complicated, the energy consumption is large, the mold requirements are high, the production efficiency is low, and the production cost is increased. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention aims to provide a highly wear-resistant and corrosion-resistant Ni-based coating and a preparation method thereof, by doping the NiAl coating with 0.05 at. % Hf to promote the formation of continuous, dense, and well-adhesive Al on the surface. 2 O 3 layer, providing excellent resistance to high-temperature oxidation, greatly improving the hardness and wear resistance of the material, giving the material good high-temperature mechanical properties and extending its service life.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] A highly wear-resistant and corrosion-resistant Ni-based coating, wherein the element composition of the Ni-based coating comprises: in atomic percentage, 49.5 at. % Al, 0.05 at. % Hf, and the remainder Ni;

[0007] The phase composition of the Ni-based coating includes Al 2 O 3 ,β-NiAl,γ′-Ni 3 Al, HfO 2 At least one of .

[0008] Preferably, the thickness of the Ni-based coating is in the range of 15 to 25 μm.

[0009] The present invention also provides a method for preparing a highly wear-resistant and corrosion-resistant Ni-based coating, comprising the following steps:

[0010] S1. Target material preparation: preparing NiAlHf target material according to the atomic percentage content of Al, Hf and Ni;

[0011] S2. Selecting a substrate: selecting a high-temperature alloy substrate and pretreating the surface of the high-temperature alloy substrate;

[0012] S3. Depositing NiAlHf coating: placing the high temperature alloy substrate into a deposition furnace, and using arc ion plating to deposit the NiAlHf coating on the surface of the high temperature alloy substrate. After vacuum heat treatment of the NiAlHf coating, a highly wear-resistant and corrosion-resistant Ni-based coating is obtained.

[0013] Preferably, in step S2, the surface of the high-temperature alloy substrate is pretreated by first grinding and polishing the surface of the high-temperature alloy substrate with sandpaper, and then ultrasonically cleaning and drying the high-temperature alloy substrate with acetone and alcohol in sequence to remove the oxide layer, impurities and adhesions on the surface of the high-temperature alloy substrate.

[0014] Preferably, in step S3, before placing the high temperature alloy substrate into the deposition furnace, the process further includes performing high pressure ion cleaning on the interior of the deposition furnace. The conditions for the high pressure ion cleaning are: the furnace is evacuated to a vacuum of 5×10 -3 Pa, furnace pressure 1.1 Pa, Ar gas flow rate 300 sccm, furnace negative bias 500-900 V.

[0015] Preferably, in step S3, the conditions of the arc ion plating method include: a deposition furnace pressure of 1.0 Pa, a high-temperature alloy substrate temperature of 300° C., an arc target current of 100 A, a high-temperature alloy substrate negative bias of 50 V, and a duty cycle of 70%.

[0016] Preferably, the high-temperature alloy substrate is CMSX-4 nickel-based high-temperature alloy.

[0017] Preferably, the method further comprises subjecting the highly wear-resistant and corrosion-resistant Ni-based coating after the NiAlHf layer is deposited to a vacuum heat treatment at 950° C. for 6 h.

[0018] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:

[0019] (1) The present invention doped 0.05 at.% Hf on the basis of NiAl coating to increase the adhesion between the oxide layer and the coating, reduce the growth rate of the oxide layer, and obtain Al with better protection and longer life. 2 O 3 layer.

[0020] (2) The NiAlHf coating used in the present invention can form a dense and continuous Al 2 O 3 Layer, Al 2 O 3 It has excellent wear resistance, corrosion resistance, high temperature resistance and other properties. Therefore, the coating can not only provide good high temperature oxidation resistance, but also enhance its wear resistance. 2 O 3 The layer can not only avoid the problems of poor wettability and weak bonding between the hard phase and the substrate in the traditional external addition method, but also solve the problem of defects such as cracks and pores in the hard phase during the cladding process.

[0021] (3) Compared with the preparation of ceramic particle reinforced and toughened NiAl intermetallic compound composite materials by mechanical alloying, hot pressing exothermic reaction synthesis, hot pressing sintering and hot pressing reaction synthesis, the arc ion plating technology used in the present invention has a fast deposition speed, a high ionization rate, simple equipment and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 This is a flow chart of a method for preparing a highly wear-resistant and corrosion-resistant Ni-based coating according to the present invention;

[0024] Figure 2 A cross-sectional view of a highly wear-resistant and corrosion-resistant Ni-based coating provided in Example 1 of the present invention at 20 μm;

[0025] Figure 3 This is a friction and wear curve diagram of the highly wear-resistant and corrosion-resistant Ni-based coating provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The highly wear-resistant and corrosion-resistant Ni-based coating provided by the present invention and its preparation method and application are described below.

[0028] NiAl intermetallic compounds have low density (5.86 g / cm 3 ), high melting point (1638℃), good thermal conductivity, high oxidation resistance and other advantages, and has been developed and applied in the field of high-temperature structural materials. The wide composition ratio range in the NiAl alloy phase diagram provides great possibilities for changing its performance. Therefore, many studies have begun to explore the use of alloying to optimize its room temperature plasticity, hardness, corrosion resistance and other properties, and strive to expand the application of NiAl intermetallic compounds in social production and engineering. Doping 0.05 at. % Hf in the NiAl coating will form fine and dispersed "oxide plugs" at the interface between the oxide layer and the coating to improve the adhesion of the oxide layer. The addition of Hf element enables the coating to obtain the expected excellent oxidation resistance and corrosion resistance. The high hardness, low surface roughness, good oxidation resistance and good adhesion between the NiAl coating and the substrate are the main reasons for the good wear resistance of the coating.

[0029] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] Embodiment 1

[0031] like Figure 1 As shown, the present invention provides a method for preparing a highly wear-resistant and corrosion-resistant Ni-based coating, comprising the following steps:

[0032] S1. Target material preparation: preparing NiAlHf target material according to the atomic percentage content of Al, Hf and Ni;

[0033] S2. Selecting a substrate: selecting a high-temperature alloy substrate and pretreating the surface of the high-temperature alloy substrate;

[0034] S3, depositing a NiAlHf layer: placing the high-temperature alloy substrate into a deposition furnace, and using an arc ion plating method to deposit the NiAlHf coating on the surface of the high-temperature alloy substrate, and subjecting the NiAlHf coating to vacuum heat treatment to obtain a highly wear-resistant and corrosion-resistant Ni-based coating.

[0035] Specifically, the atomic percentage contents of the above-mentioned Al, Hf and Ni are: 49.5 at. % Al, 0.05 at. % Hf, and the rest is Ni.

[0036] Among them, in step S2, the surface of the high-temperature alloy substrate is pretreated as follows: first, the surface of the high-temperature alloy substrate is grinded and polished with sandpaper, and then the high-temperature alloy substrate is ultrasonically cleaned and dried with acetone and alcohol in sequence to remove the oxide layer, impurities and adhesions on the surface of the high-temperature alloy substrate.

[0037] Specifically, in step S3, before placing the high-temperature alloy substrate into the deposition furnace, the interior of the deposition furnace is subjected to high-pressure ion cleaning. The conditions for high-pressure ion cleaning are: the furnace is evacuated to 5×10 -3 Pa, furnace pressure 1.1 Pa, Ar gas flow rate 300 sccm, furnace negative bias 650 V.

[0038] In addition, the conditions of the arc ion plating method include: a deposition furnace pressure of 1.0 Pa, a high-temperature alloy substrate temperature of 300°C, an arc target current of 100 A, a high-temperature alloy substrate negative bias of 50 V, and a duty cycle of 70%. Among them, the above-mentioned high-temperature alloy substrate is preferably the second-generation nickel-based high-temperature alloy CMSX-4. Compared with the preparation of ceramic particle reinforced and toughened NiAl intermetallic compound composites by mechanical alloying, hot pressing exothermic reaction synthesis, hot pressing sintering and hot pressing reaction synthesis, this embodiment adopts an arc ion plating method, which has a fast deposition speed, a high ionization rate, simple equipment and low cost. In addition, Al is generated in situ by high-temperature oxidation on the surface of the NiAlHf coating. 2 O 3 The layer can not only avoid the problems of poor wettability and weak bonding between the hard phase and the substrate in the traditional external addition method, but also solve the problem of defects such as cracks and pores in the hard phase during the cladding process. Figure 2 The NiAlHf coating was prepared by arc ion plating. The structure between the NiAlHf coating and the base alloy was dense, and no defects such as cracks and pores were found. In addition, the coating preparation equipment was simple and the process was controllable. The prepared coating had good interface bonding with the base alloy.

[0039] More specifically, in step S3, the highly wear-resistant and corrosion-resistant Ni-based coating after the NiAlHf layer is deposited is further subjected to vacuum heat treatment at 950° C. for 6 h.

[0040] The phase composition of the highly wear-resistant and corrosion-resistant Ni-based coating prepared according to the above preparation method includes Al 2 O 3 ,β-NiAl,γ′-Ni 3 Al, HfO2 and measured to have a thickness of approximately 20 μm.

[0041] In addition, refer to Figure 3 From the friction and wear curve of the Ni-based coating, it can be seen that due to the formation of a dense and continuous aluminum oxide layer on the surface of the Ni-based coating, the wear rate W of the prepared Ni-based coating is 1.779×10 -14 m 3 / (N·m), which proves that the Ni-based coating prepared by the above method in this embodiment has good corrosion resistance and wear resistance.

[0042] Therefore, the above-mentioned high wear-resistant and corrosion-resistant Ni-based coating and its preparation method are adopted, and the NiAl coating is doped with 0.05 at.% Hf to promote the formation of continuous, dense, and well-adhered Al on the surface. 2 O 3 layer, providing excellent resistance to high-temperature oxidation, greatly improving the hardness and wear resistance of the material, giving the material good high-temperature mechanical properties and extending its service life.

[0043] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing a highly wear-resistant and corrosion-resistant Ni-based coating, characterized in that: The element composition of the Ni-based coating includes: in atomic percentage, 49.5 at.% Al, 0.05 at.% Hf, and the remainder Ni; The phase composition of the Ni-based coating includes at least one of Al2O3, β-NiAl, γ′-Ni3Al, and HfO2; the thickness of the Ni-based coating ranges from 15 to 25 μm; The preparation method of the Ni-based coating comprises the following steps: S1. Target material preparation: preparing NiAlHf target material according to the atomic percentage content of Al, Hf and Ni; S2. Selecting a substrate: selecting a high-temperature alloy substrate and pretreating the surface of the high-temperature alloy substrate; the high-temperature alloy substrate is a second-generation nickel-based high-temperature alloy CMSX-4; S3, depositing NiAlHf coating: placing the high temperature alloy substrate into a deposition furnace, and using arc ion plating to deposit the NiAlHf coating on the surface of the high temperature alloy substrate, and subjecting the NiAlHf coating to vacuum heat treatment to obtain a highly wear-resistant and corrosion-resistant Ni-based coating; In step S3, before placing the high temperature alloy substrate into the deposition furnace, the deposition furnace is subjected to high pressure ion cleaning. The conditions for the high pressure ion cleaning are as follows: the furnace is evacuated to a vacuum of 5×10 -3 Pa, furnace pressure 1.1Pa, Ar gas flow rate 300sccm, furnace negative bias 500-900V; the conditions of the arc ion plating method include: deposition furnace pressure 1.0Pa, high temperature alloy substrate temperature of 300°C, arc target current 100A, high temperature alloy substrate negative bias 50V, duty cycle 70%; the above process also includes vacuum heat treatment of the highly wear-resistant and corrosion-resistant Ni-based coating after depositing the NiAlHf layer at 950°C for 6h.

2. The method for preparing a highly wear-resistant and corrosion-resistant Ni-based coating according to claim 1, characterized in that: In step S2, the surface of the high-temperature alloy substrate is pretreated by first grinding and polishing the surface of the high-temperature alloy substrate with sandpaper, and then ultrasonically cleaning and drying the high-temperature alloy substrate with acetone and alcohol in sequence to remove the oxide layer, impurities and adhesions on the surface of the high-temperature alloy substrate.