A single crystal furnace and growth method for reducing silicon liquid oxygen content and heating power

By using lifting and lowering insulation components in the production of single crystal silicon, the temperature gradient of the cold and hot zones is adjusted, and the problems of affected airflow flow and high oxygen content are solved, and the effect of improving crystal growth speed and extending the life of the equipment is achieved.

CN118563410BActive Publication Date: 2024-11-19苏州晨晖智能设备有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411000908.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-19
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In the existing single crystal silicon production technology, the method of increasing the supercooling degree of the cold zone will affect the airflow flow in the single crystal furnace, the service life of water-cooled parts and heat-insulating parts is short, and the oxygen content in the single crystal silicon is high, affecting the crystal. quality.

Method used

A single crystal furnace design and growth method is adopted, including setting up a lifting and insulation component on the outside of the crucible, setting the insulation block along the circumference of the crucible wall, and the lifting drive member drives the insulation block to move up and down, adjusting the temperature gradient of the cold and hot zones, and reducing heating. Power prevents the flow of the air flow from affecting the airflow, and controls the position of the insulation block and the heating power of the heating part to inhibit the entry of oxygen elements into the silicon liquid.

Benefits of technology

It improves the crystal growth speed and efficiency, extends the service life of the components in the single crystal furnace, reduces the oxygen content of the single crystal silicon, and improves the crystal quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563410B_ABST
    Figure CN118563410B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of single crystal silicon production, and specifically relates to a single crystal furnace and a growth method for reducing the oxygen content and heating power of silicon liquid. The single crystal furnace includes a furnace body, and also includes: a crucible, which is arranged in the furnace body, and its crucible wall is arranged along the circumference of the furnace body wall, and the cavity inside it is used to accommodate silicon material; an insulation cylinder, which is arranged in the furnace body and located on the outside of the crucible, and is arranged along the circumference of the crucible wall; a heating part, which is arranged in the insulation cylinder, and is used to heat the silicon material in the crucible; a lifting and insulation assembly, which is arranged in the furnace body and located on the outside of the crucible, and includes an insulation block and a lifting drive, the insulation block is a tubular structure and is arranged along the circumference of the crucible wall, the lifting drive is connected to the insulation block, and the lifting drive drives the insulation block to move up and down. While increasing the supercooling degree of the cold zone, it avoids affecting the airflow, the service life of the corresponding components is long, and the oxygen content in the single crystal silicon is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of single crystal silicon production, and in particular relates to a single crystal furnace and a growth method for reducing the oxygen content of silicon liquid and the heating power. Background Art

[0002] Monocrystalline silicon is an important material for preparing solar cells in the photovoltaic industry. It is usually prepared by the direct pulling method. Specifically, a block of silicon material is placed in a crucible, the silicon material is heated to the melting point to melt it, and under the protection of an inert gas, a seed crystal is used as a seed to pull it into a single crystal silicon rod.

[0003] During the crystal pulling process in a single crystal furnace, a temperature gradient is required below the surface of the silicon liquid and around and above the surface of the silicon liquid to grow the crystal rod. Currently, the main method of increasing the supercooling degree of the cold zone above the surface of the silicon liquid is to increase the crystal pulling speed and the crystal growth efficiency. The existing technology mainly increases the supercooling degree of the cold zone by setting water cooling components and heat insulation components between the guide tube and the crystal rod to increase the crystal growth speed. However, the setting of water cooling components and heat insulation components will affect the air flow in the single crystal furnace, etc., which will affect the crystal growth process. The mechanical structure of the water cooling components and heat insulation components is complex. Due to the high temperature in the center of the upper part of the crucible, the service life of the water cooling components and heat insulation components is short. In addition, in the current process of preparing single crystal silicon by the Czochralski method, the oxygen content in the single crystal silicon is relatively high, which affects the quality of the crystal.

[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the existing method of increasing the supercooling degree of the cold zone, such as the airflow circulation in the single crystal furnace is affected, the service life of the water cooling components and the insulation components is short, and the oxygen content of the single crystal silicon is relatively high. A single crystal furnace and a growth method for reducing the oxygen content of silicon liquid and the heating power are provided. While increasing the supercooling degree of the cold zone, the airflow circulation is avoided from being affected, the service life of the corresponding components is long, and the oxygen content in the single crystal silicon is reduced.

[0006] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a single crystal growth method for reducing the oxygen content of silicon liquid and the heating power, which is carried out in a single crystal furnace, wherein the single crystal furnace comprises a furnace body and further comprises:

[0007] A crucible is arranged in the furnace body, the crucible wall of which is arranged along the circumference of the furnace body wall, and the cavity inside the crucible is used to contain silicon material;

[0008] A heat preservation cylinder is arranged in the furnace body and outside the crucible, and is arranged along the circumference of the crucible wall;

[0009] A heating unit, which is disposed in the heat-insulating cylinder and is used to heat the silicon material in the crucible;

[0010] A lifting and heat-insulating assembly is arranged in the furnace body and outside the heat-insulating cylinder, and comprises a heat-insulating block and a lifting and driving member, wherein the heat-insulating block is a cylindrical structure and is arranged along the circumference of the crucible wall, and the lifting and driving member is connected to the heat-insulating block, and the lifting and driving member drives the heat-insulating block to move up and down;

[0011] The single crystal growth method comprises: loading silicon material into a crucible, placing a heat preservation block above silicon liquid at the beginning of an equal-diameter growth stage, gradually moving the crucible upward during the equal-diameter growth stage, and driving the heat preservation block to gradually move downward by a lifting drive;

[0012] The growth conditions of the isodiametric growth stage include:

[0013] The single crystal growth length is L 单晶 , L 单晶 The unit is mm, and the vertical distance between the position of the insulation block and the position of the insulation block at the beginning of the equal diameter growth stage is D 保温块 , D 保温块 = k 1× L 单晶 , k 1 is 0.05~0.07;

[0014] When the lower end of the heat-insulating block is lower than the liquid level of the silicon liquid in the crucible, the heating power of the heating part is 2kw-3kw lower than the heating power when the lifting and heat-insulating assembly is not provided.

[0015] Preferably, when the single crystal growth length is less than 300 mm, k 1 is 0.062~0.07; when the single crystal growth length is greater than 300mm, k 1 is 0.05~0.06.

[0016] Preferably, the growth conditions in the equal-diameter growth stage further include: a crucible rotation speed of 4 rpm to 6.5 rpm, a crystal rotation speed of 6 rpm to 10 rpm, and a crystal pulling speed of 70 mm / h to 110 mm / h.

[0017] Preferably, when the single crystal growth length is less than 300 mm, the crucible rotation speed is 4 rpm to 5 rpm, and when the single crystal growth length is greater than 300 mm, the crucible rotation speed remains constant, and the crucible rotation speed is 5.5 rpm to 6.5 rpm.

[0018] Preferably, when the single crystal growth length is less than 300 mm, the crystal rotation speed is 8 rpm to 10 rpm, and when the single crystal growth length is greater than 300 mm, the crystal rotation speed is 6 rpm to 7 rpm.

[0019] Preferably, when the single crystal growth length is less than 300 mm, the crystal pulling speed is 70 mm / h to 90 mm / h, and when the single crystal growth length is greater than 300 mm, the crystal pulling speed is 95 mm / h to 110 mm / h.

[0020] Preferably, the growth conditions in the isodiameter growth stage further include: the pressure in the single crystal furnace is 11 torr to 13 torr.

[0021] The single crystal furnace of the present invention comprises a furnace body, wherein a crucible is arranged in the furnace body and the crucible wall is arranged along the circumference of the furnace body wall, an insulation cylinder is arranged along the circumference of the crucible wall on the outside of the crucible in the furnace body, a heating part for heating silicon material in the crucible is arranged in the insulation cylinder, and a lifting and insulation assembly including an insulation block and a lifting drive member is arranged on the outside of the crucible in the furnace body, the insulation block is a tubular structure and is arranged along the circumference of the crucible wall, and the lifting drive member drives the insulation block to move up and down. During the single crystal growth process, silicon material is loaded into the crucible. At the beginning of the equal-diameter growth stage, the insulation block is located above the silicon liquid. During the equal-diameter growth stage, the lifting drive drives the insulation block to move gradually downward, which can gradually improve the heat dissipation capacity of the cold zone above the surface of the silicon liquid, improve the supercooling of the cold zone, promote the crystal growth process, and improve the crystal growth speed and efficiency. Since the insulation block moves downward, the insulation capacity of the hot zone below the surface of the silicon liquid can be improved, and the heating power of the heating part can be reduced. Since the heating power is reduced, the crucible rotation speed can be appropriately reduced, the oxygen element is inhibited from entering the silicon liquid, the oxygen content of the single crystal silicon is reduced, the quality of the single crystal silicon is improved, and defects are reduced.

[0022] The arrangement of the lifting and heat-insulating component of the present invention will not affect the airflow in the single crystal furnace, and will not affect the crystal growth due to the influence on the airflow. At the same time, the lifting and heat-insulating component is located closer to the outside of the furnace body, the temperature is relatively low, the heat is less, and the service life is long. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 It is a schematic cross-sectional structure diagram of an embodiment of a single crystal furnace of the present invention.

[0025] Description of Reference Numerals

[0026] 1. Furnace body; 2. Crucible; 3. Insulation tube; 4. Heating part; 5. Lifting and insulation assembly; 501. Insulation block; 502. Lifting drive member. DETAILED DESCRIPTION

[0027] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0028] In this document, unless otherwise specified, directional words such as "upper" and "lower" are generally understood in combination with the directions shown in the drawings and actual applications, and "inside" and "outside" refer to the inside and outside of the outline of a component.

[0029] In the description of the present invention, it is necessary to understand that the terms "center", "length", "thickness", "up", "down", "vertical", "inside", "outside", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0030] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0031] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0032] The inventors of the present invention have found that the existing method of increasing the degree of supercooling in the cold zone affects the airflow in the single crystal furnace, shortens the service life of water-cooling components and heat-insulating components, and produces a high oxygen content in the prepared single crystal silicon.

[0033] In this regard, in a first aspect, the present invention provides a single crystal growth method for reducing the oxygen content of silicon liquid and the heating power, which is performed in a single crystal furnace, wherein the single crystal furnace comprises a furnace body 1, and further comprises:

[0034] A crucible 2 is disposed in the furnace body 1, wherein the crucible wall is disposed along the circumference of the furnace body wall, and the cavity therein is used to contain silicon material;

[0035] A heat preservation tube 3, which is arranged in the furnace body 1 and located outside the crucible 2, and is arranged along the circumference of the crucible wall;

[0036] A heating unit 4 is disposed in the heat preservation tube 3 and is used to heat the silicon material in the crucible 2;

[0037] A lifting and heat-insulating assembly 5, which is arranged in the furnace body 1 and located outside the heat-insulating cylinder 3, comprises a heat-insulating block 501 and a lifting and driving member 502, wherein the heat-insulating block 501 is a cylindrical structure and is arranged along the circumference of the crucible wall, and the lifting and driving member 502 is connected to the heat-insulating block 501, and the lifting and driving member 502 drives the heat-insulating block 501 to move up and down;

[0038] The growth method includes: loading silicon material into a crucible, placing a heat preservation block 501 above the silicon liquid at the beginning of an equal-diameter growth stage, gradually moving the crucible 2 upwards during the equal-diameter growth stage, and driving the heat preservation block 501 to gradually move downwards by a lifting drive 502;

[0039] The growth conditions of the isodiametric growth stage include:

[0040] The single crystal growth length is L 单晶 , L 单晶 The unit is mm, and the vertical distance between the position of the insulation block 501 and the position of the insulation block 501 at the beginning of the equal diameter growth stage is D 保温块 , D 保温块 = k 1× L 单晶 , k 1 is 0.05~0.07;

[0041] When the lower end of the heat preservation block 501 is lower than the liquid level of the silicon liquid in the crucible 2, the heating power of the heating part 4 is 2kw-3kw lower than the heating power when the lifting and heat preservation component 5 is not provided. The heating power when the lifting and heat preservation component is not provided refers to the heating power required to achieve the same heating temperature when the lifting and heat preservation component is not provided, which can be obtained by historical data, theoretical calculation, etc.

[0042] A crucible is arranged in the furnace body of the present invention, and the crucible wall is arranged along the circumference of the furnace body wall. A heat preservation cylinder is arranged on the outer side of the crucible in the furnace body and along the circumference of the crucible wall. A heating part for heating silicon material in the crucible is arranged in the heat preservation cylinder. A lifting and insulation assembly including a heat preservation block and a lifting and insulation driving part is arranged on the outer side of the crucible in the furnace body. The heat preservation block is a tubular structure arranged along the circumference of the crucible wall. The lifting and insulation driving part is connected to the heat preservation block, and the lifting and insulation driving part drives the heat preservation block to move up and down. By setting the dual insulation structure of the fixed insulation cylinder 3 and the movable lifting and insulation assembly, when growing silicon carbide single crystals, at the beginning of the equal-diameter growth stage, the insulation block is located above the silicon liquid, and in the equal-diameter growth stage, the crucible is gradually moved upward, and the lifting drive drives the insulation block to gradually move downward. By gradually moving the insulation block downward, the heat dissipation capacity of the cold zone above the surface of the silicon liquid can be gradually improved, the supercooling of the cold zone can be improved, and the temperature gradient between the cold zone above the surface of the silicon liquid and the hot zone below the surface of the silicon liquid can be increased, so as to promote the crystal growth process, increase the crystal growth and crystal pulling speed, and increase the production capacity. The lifting and insulation assembly of the present invention is located outside the crucible. Compared with adding water cooling and heat insulation components between the guide cylinder and the crystal rod, on the one hand, it avoids affecting the air flow in the furnace, etc., and avoids affecting the crystal growth. On the other hand, it receives less heating from the heating part, receives less heat, and has a long service life of the lifting and insulation assembly. When the lifting and insulation assembly 5 is located outside the insulation cylinder 3, the lifting and insulation assembly receives less heating from the heating part, receives less heat, and has a longer service life.

[0043] In the present invention, during the isodiameter growth stage, the insulation block moves downward, which can improve the insulation capacity of the hot zone below the surface of the silicon liquid. Under the premise of maintaining the same temperature distribution, it can reduce the power loss in the crystal pulling process, reduce the heating power of the heating part, and reduce energy consumption. Since the heating power is reduced, the heating non-uniformity is lower, and the crucible rotation speed can be appropriately reduced, thereby reducing the fluidity of the melt, inhibiting the entry of oxygen into the silicon liquid, reducing the oxygen content of the single crystal silicon, improving the quality of the single crystal silicon, and reducing defects.

[0044] In addition, the provision of the lifting and heat preservation assembly of the present invention increases the control and adjustment dimension of the crystal pulling process. The present invention does not limit the form of the lifting and heat preservation drive member, and it only needs to enable the heat preservation block 501 to perform lifting and heat preservation movement.

[0045] According to the single crystal growth method of the present invention, at the beginning of the equal-diameter growth stage, the insulation block is located above the silicon liquid. During the equal-diameter growth stage, the lifting drive member drives the insulation block to gradually move downward, which can gradually improve the heat dissipation capacity of the cold zone above the silicon liquid surface, improve the supercooling of the cold zone, increase the temperature gradient between the cold zone above the silicon liquid surface and the hot zone below the silicon liquid surface, promote the crystal growth process, increase the crystal growth and crystal pulling speeds, and increase production capacity. It can improve the insulation capacity of the hot zone below the silicon liquid surface, reduce the heating power of the heating part, appropriately reduce the crucible rotation speed, and inhibit the entry of oxygen into the silicon liquid by reducing the fluidity of the melt, thereby reducing the oxygen content of the single crystal silicon, improving the quality of the single crystal silicon, and reducing defects.

[0046] The vertical distance between the position of the insulation block 501 and the position of the insulation block 501 at the beginning of the equal diameter growth stage D 保温块 for k 1 and single crystal growth length L 单晶 The product of the heat preservation block is controlled according to the crystal growth length, which is more conducive to improving the heat dissipation capacity of the cold zone above the silicon liquid surface and improving the heat preservation capacity of the hot zone below the silicon liquid surface. The process matches the crystal growth process, improves the crystal quality, and reduces the oxygen content. k 1 is 0.05-0.07, which is more conducive to improving the quality of the crystal and reducing the oxygen content. When the lower end of the insulation block is lower than the liquid level of the silicon liquid in the crucible, the heating power of the heating part is 2kw-3kw lower than the heating power when the lifting insulation component is not set, which is more conducive to improving the quality of the single crystal silicon crystal.

[0047] Preferably, when the single crystal growth length is less than 300 mm, k 1 is 0.062~0.07; when the single crystal growth length is greater than 300mm, k 1 is 0.05-0.06. Under this preferred embodiment, in the early stage of crystal growth, k 1 is 0.062~0.07. According to the growth length, a faster downward movement speed of the heat preservation block is adopted, which is more conducive to accelerating the cooling of the crystal rod, increasing the growth rate of the crystal rod, reducing the fluctuation of the oxygen content in the diameter of the crystal rod in the early stage of equal diameter growth, and improving the quality of the crystal rod; in the later stage of equal diameter growth of the crystal, k 1 is 0.05~0.06. According to the growth length, a slower downward movement speed of the insulation block is adopted to achieve a smooth change in the insulation performance of the hot zone, which is more conducive to reducing the temperature fluctuation of the hot zone and improving the quality of the crystal rod.

[0048] Preferably, the growth conditions of the equal-diameter growth stage also include: the crucible rotation speed is 4rpm~6.5rpm, the crystal rotation speed is 6rpm~10rpm, and the crystal pulling speed is 70mm / h~110mm / h. Under this preferred scheme, combined with the heating power of the heating part being 2kw-3kw lower than the heating power when the lifting and heat-insulating component is not provided, the crucible rotation speed is 4rpm~6.5rpm, which is more conducive to reducing the fluidity of the melt in the crucible, reducing the probability of oxygen elements entering the silicon solution, reducing the oxygen content of single crystal silicon, and improving the quality of single crystal silicon under the premise of ensuring uniform heating all around the crucible; the crystal rotation speed is 6rpm~10rpm, which is more conducive to reducing the fluidity of the melt, reducing the probability of oxygen elements entering the silicon solution, reducing the oxygen content, and improving the quality of single crystal silicon. The crystal pulling speed is 70mm / h~110mm / h, and the vertical distance between the position of the heat-insulating block 501 and the position of the heat-insulating block 501 at the beginning of the equal-diameter growth stage. D 保温块 for k 1 and single crystal growth length L 单晶 The product of k 1 is matched with 0.05~0.07, which is more conducive to the stable equal-diameter growth of the crystal, and the equal-diameter growth process goes smoothly, thereby improving the crystal quality.

[0049] Preferably, when the single crystal growth length is less than 300mm, the crucible speed is 4rpm~5rpm, and when the single crystal growth length is more than 300mm, the crucible speed remains constant, and the crucible speed is 5.5rpm~6.5rpm. Under this preferred scheme, when the growth length is less than 300mm, the crucible speed is 4rpm~5rpm, and a smaller crucible rotation speed is used, which is conducive to reducing the probability of oxygen entering the silicon solution, reducing the oxygen content, reducing the fluctuation of the oxygen content of the crystal rod in the early stage of equal diameter, and improving the quality of the crystal rod; when the growth length is more than 300mm, the crucible speed is 5.5rpm~6.5rpm, and a constant and smaller crucible rotation speed is used, which is more conducive to reducing the oxygen content, reducing the melt fluctuation, reducing the fluctuation of the oxygen content of the crystal rod, and improving the quality of the crystal rod.

[0050] Preferably, when the single crystal growth length is less than 300 mm, the crystal rotation speed is 8 rpm to 10 rpm, and when the single crystal growth length is more than 300 mm, the crystal rotation speed is 6 rpm to 7 rpm. Under this preferred scheme, it is more conducive to reducing the oxygen content while reducing melt fluctuations, reducing crystal rod oxygen content fluctuations, and improving crystal rod quality.

[0051] Preferably, when the single crystal growth length is less than 300 mm, the crystal pulling speed is 70 mm / h to 90 mm / h, and when the single crystal growth length is greater than 300 mm, the crystal pulling speed is 95 mm / h to 110 mm / h. Under this preferred solution, it is more conducive to the stable equal-diameter growth of the crystal, the equal-diameter growth process proceeds smoothly, the crystal quality is improved, and the production efficiency is improved.

[0052] Preferably, the growth conditions of the equal diameter growth stage also include: the pressure in the single crystal furnace is 11torr~13torr and the pressure value is kept constant. Under this preferred solution, the pressure is 11torr~13torr, and the pressure value is kept constant, which is more conducive to the smooth and smooth equal diameter growth, reduces the difficulty of airflow control, and moves the insulation block to adjust the control.

[0053] The present invention is further described in detail below with reference to specific embodiments.

[0054] Example 1

[0055] A single crystal furnace, see Figure 1 , including a furnace body, a crucible 2, a heat preservation tube 3, a heating part 4 and a lifting and heat preservation assembly 5; the crucible 2 is arranged in the furnace body 1, the crucible wall is arranged along the circumference of the furnace body wall, and the cavity in the crucible is used to contain silicon material; the heat preservation tube 3 is arranged in the furnace body 1 and located on the outside of the crucible 2, and the heat preservation tube 3 is arranged along the circumference of the crucible wall; the heating part 4 is arranged in the heat preservation tube 3, and is used to heat the silicon material in the crucible 2; the lifting and heat preservation assembly 5 is arranged in the furnace body 1 and located on the outside of the heat preservation tube 3, and the lifting and heat preservation assembly 5 includes a heat preservation block 501 and a lifting drive 502, the heat preservation block 501 is a tubular structure and is arranged along the circumference of the crucible wall, the lifting drive 502 is connected to the heat preservation block 501, and the lifting drive 502 drives the heat preservation block 501 to move up and down. The thickness of the heat preservation block is 40mm and the height is 300mm.

[0056] A single crystal growth method is carried out in the above-mentioned single crystal furnace, including loading silicon material into a crucible, and at the beginning of the equal-diameter growth stage, positioning the insulation block 501 above the silicon liquid. During the equal-diameter growth stage, the crucible 2 is gradually moved upward, and the lifting drive 502 drives the insulation block 501 to gradually move downward.

[0057] In the isodiameter growth stage, the pressure in the single crystal furnace is maintained at 12 torr. L 单晶 , L 单晶 The unit is mm, and the vertical distance between the position of the insulation block 501 and the position of the insulation block 501 at the beginning of the equal diameter growth stage is D 保温块 , D 保温块 =k 1× L 单晶 , when the single crystal growth length is less than 300mm, k 1 is 0.062~0.07, when the single crystal growth length is greater than 300mm, k 1 is 0.05~0.06, controlling the position of the insulation block 501, L 单晶 80mm, D 保温块 5mm( k 1 is 0.0625), L 单晶 150mm, D 保温块 10mm( k 1 is 0.0667), L 单晶 300mm, D 保温块 20mm( k 1 is 0.0667), L 单晶 500mm, D 保温块 30mm( k 1 is 0.06).

[0058] according to L 单晶 The crucible speed, crystal speed and crystal pulling speed are controlled. When the L single crystal is 1 mm, the crucible speed is 4 rpm, the crystal speed is 10 rpm, and the pulling speed is 70 mm / h. When the L single crystal is 80 mm, the crucible speed is 4 rpm, the crystal speed is 9 rpm, and the pulling speed is 80 mm / h. When the L single crystal is 150 mm, the crucible speed is 5 rpm, the crystal speed is 8 rpm, and the pulling speed is 90 mm / h. When the L single crystal is 300 mm, the crucible speed is 6 rpm, the crystal speed is 7 rpm, and the pulling speed is 100 mm / h. When the L single crystal is 500 mm, the crucible speed is 6 rpm, the crystal speed is 6 rpm, and the pulling speed is 100 mm / h. The oxygen content of the single crystal silicon prepared in this embodiment is 7-8 ppma.

[0059] Example 2

[0060] Referring to the single crystal growth method of Example 1, the difference is that when the single crystal growth length is less than 300 mm, k 1 is 0.05~0.06, when the single crystal growth length is greater than 300mm, k 1 is 0.062~0.07, controlling the position of the insulation block 501, L 单晶 80mm, D 保温块 4.8mm(k 1 is 0.06), L 单晶 150mm, D 保温块 9mm( k 1 is 0.06), L 单晶 300mm, D 保温块 18mm ( k 1 is 0.06), L 单晶 500mm, D 保温块 35mm ( k 1 is 0.07). The oxygen content of the single crystal silicon prepared in this embodiment is 9 ppma.

[0061] Example 3

[0062] The single crystal growth method of Example 1 is referred to, except that when the single crystal growth length is less than 300 mm, the crucible rotation speed is 6 rpm. The oxygen content of the single crystal silicon prepared in this example is 10 ppma.

[0063] Comparative Example 1

[0064] Referring to the single crystal furnace of Example 1, except that the lifting and heat preservation component 5 is not provided, referring to the single crystal growth method of Example 1, except that during equal diameter growth, according to L 单晶 Control crucible speed, crystal speed and crystal pulling speed, L 单晶 When the diameter is 1mm, the crucible is rotated at 5rpm, the crystal is rotated at 10rpm, and the pulling speed is 70mm / h. L 单晶 When the diameter is 80mm, the crucible is rotated at 5rpm, the crystal is rotated at 9rpm, and the pulling speed is 80mm / h. L 单晶 When the diameter is 150mm, the crucible is rotated at 6rpm, the crystal is rotated at 8rpm, and the pulling speed is 90mm / h. L 单晶 When the diameter is 300mm, the crucible is rotated at 7rpm, the crystal is rotated at 7rpm, and the pulling speed is 90mm / h. L 单晶 When the diameter of the silicon crystal is 500 mm, the crucible is rotated at 8 rpm, the crystal is rotated at 7 rpm, and the pulling speed is 90 mm / h. The oxygen content of the single crystal silicon prepared in this comparative example is 14 ppma.

[0065] Comparing Example 1 with Comparative Example 1, by setting the lifting and heat preservation component, the crystal pulling speed can be increased, the production capacity can be increased, the heating power can be reduced, the energy consumption can be reduced, the crucible speed can be reduced, the oxygen content of the single crystal silicon can be reduced, and the quality of the single crystal silicon can be improved. Comparing Example 1 with Example 2, when the single crystal growth length is less than 300 mm, the k 1 is 0.062~0.07; when the single crystal growth length is greater than 300mm, k 1 is 0.05-0.06, which is more conducive to obtaining high-quality crystal rods with low oxygen content. Comparing Example 1 and Example 3, when the single crystal growth length is less than 300 mm, the crucible rotation speed is 4 rpm-5 rpm, which is more conducive to obtaining crystal rods with low oxygen content.

[0066] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A single crystal growth method for reducing the oxygen content and heating power of silicon liquid, characterized in that: The process is carried out in a single crystal furnace, wherein the single crystal furnace comprises a furnace body (1) and further comprises: A crucible (2) is arranged in the furnace body (1), the crucible wall of which is arranged along the circumference of the furnace body wall, and the cavity therein is used to contain silicon material; A heat-insulating cylinder (3) arranged in the furnace body (1) and located outside the crucible (2), and arranged along the circumference of the crucible wall; A heating part (4), which is arranged in the heat-insulating cylinder (3) and is used to heat the silicon material in the crucible (2); a lifting and heat-insulating assembly (5), which is arranged in the furnace body (1) and located outside the heat-insulating cylinder (3), and comprises a heat-insulating block (501) and a lifting and heat-insulating driving member (502), wherein the heat-insulating block (501) is a cylindrical structure and is arranged along the circumference of the crucible wall, and the lifting and heat-insulating driving member (502) is connected to the heat-insulating block (501), and the lifting and heat-insulating driving member (502) drives the heat-insulating block (501) to move up and down; The single crystal growth method comprises: loading silicon material into the crucible (2), positioning the heat preservation block (501) above the silicon liquid at the beginning of the equal-diameter growth stage, gradually moving the crucible (2) upwards during the equal-diameter growth stage, and driving the heat preservation block (501) to gradually move downwards by the lifting drive member (502); The growth conditions of the isodiametric growth stage include: The single crystal growth length is L 单晶 , L 单晶 The unit is mm, and the vertical distance between the position of the insulation block (501) and the position of the insulation block (501) at the beginning of the equal-diameter growth stage is D 保温块 , D 保温块 = k 1× L 单晶 When the single crystal growth length is less than 300 mm, k 1 is 0.062~0.07, when the single crystal growth length is greater than 300mm, k 1 is 0.05~0.06; When the lower end of the heat-insulating block (501) is lower than the liquid level of the silicon liquid in the crucible (2), the heating power of the heating part (4) is 2 kW-3 kW lower than the heating power when the lifting and heat-insulating component (5) is not provided; When the single crystal growth length is less than 300 mm, the crucible rotation speed is 4 rpm to 5 rpm. When the single crystal growth length is more than 300 mm, the crucible rotation speed is kept constant, and the crucible rotation speed is 5.5 rpm to 6.5 rpm.

2. The single crystal growth method according to claim 1, characterized in that: The growth conditions of the equal-diameter growth stage also include: a crystal rotation speed of 6 rpm to 10 rpm, and a crystal pulling speed of 70 mm / h to 110 mm / h.

3. The single crystal growth method according to claim 2, characterized in that: When the single crystal growth length is less than 300 mm, the crystal rotation speed is 8 rpm to 10 rpm. When the single crystal growth length is greater than 300 mm, the crystal rotation speed is 6 rpm to 7 rpm.

4. The single crystal growth method according to claim 2, characterized in that: When the single crystal growth length is less than 300 mm, the crystal pulling speed is 70 mm / h to 90 mm / h. When the single crystal growth length is greater than 300 mm, the crystal pulling speed is 95 mm / h to 110 mm / h.

5. The single crystal growth method according to claim 2, characterized in that: The growth conditions of the isodiameter growth stage also include: the pressure in the single crystal furnace is 11 torr to 13 torr.