A drag reducing agent for fracturing and preparation method thereof
Through the polymerization preparation of modified monomers and additives, the drag reduction performance of the drag reduction agent is improved, the problem of large friction resistance of the fluid in slippery water fracturing is solved, and more efficient flow and energy utilization is achieved.
Patent Information
- Application Number
- CN202410816245.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-06-24
AI Technical Summary
At this stage, the drag reduction effect of the drag reduction agent is average, resulting in large friction resistance of the fluid during the slippery water fracturing process, affecting flow efficiency and energy consumption.
The drag reducing agent is prepared by polymerizing the modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and octadecanoate under specific conditions, and the drag reducing agent is prepared by silicone The chain segment improves rigidity and hydrophobic effects, and avoids the hydration and expansion of formation clay minerals through nano-inorganic substances, thereby increasing the ability to carry sand.
The drag reduction performance of the drag reducing agent is significantly improved, the friction resistance of the fluid in the pipeline is reduced, and the output and energy utilization of the fracturing fluid are improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of drag reducer preparation, and in particular to a drag reducer for fracturing and a preparation method thereof. Background Art
[0002] Shale gas reservoirs are characterized by low porosity and low permeability. Currently, slick water hydraulic fracturing technology and horizontal well technology are mainly used for exploitation. Slick water fracturing transformation technology mainly changes the conductivity of low permeability reservoirs and increases their permeability, so as to achieve the purpose of increasing oil and production. Slick water hydraulic fracturing technology pressurizes the fracturing fluid by high-pressure pump injection equipment and then pumps it into the formation at high speed through the tubing. Under high pressure and high speed conditions, the turbulence phenomenon is serious during the flow of the fluid in the pipe, and there is a large friction resistance between the fracturing fluid and the pipe wall. The friction resistance of the fluid limits the flow of the fluid in the pipeline, resulting in a decrease in pipeline output and an increase in energy loss. Therefore, the core part of the slick water fracturing fluid is the preparation of the base fluid, which requires the drag reducer to have good performance indicators. Summary of the invention
[0003] The purpose of the present invention is to provide a drag reducer for fracturing and a preparation method thereof, which solves the problem that the drag reducing effect of the current drag reducer is mediocre.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A method for preparing a drag reducer for fracturing, comprising the following steps:
[0006] The modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, octadecyl methacrylate and DMF are uniformly mixed, nitrogen is introduced for protection, potassium persulfate is added and stirred at a speed of 120-150 r / min and a temperature of 25-30° C., and the mixture is reacted for 4-6 hours to obtain a drag reducer for fracturing.
[0007] Furthermore, the amount ratio of the modified monomer, the modified additive, acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid and methacrylate octadecyl is 3 mol:50g:75 mol:20 mol:5 mol:0.04 mol, and the amount of potassium persulfate is 0.05% of the total mass of the modified monomer, the modified additive, acrylamide, sodium p-styrene sulfonate, 2-acrylamide-2-methylpropane sulfonic acid and methacrylate octadecyl.
[0008] Further, the modified monomer is prepared by the following steps:
[0009] Step A1: β-cyclodextrin, sodium hydroxide and deionized water are mixed, stirred and sodium chloroacetate is added at a speed of 120-150 r / min and a temperature of 25-30° C., and the reaction is carried out for 3-5 hours, and the pH value is adjusted to 5 to obtain carboxymethyl cyclodextrin; carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane, dicyclohexylcarbodiimide and toluene are mixed, and the reaction is carried out at a speed of 60-80 r / min and a temperature of 40-50° C. for 6-8 hours to obtain modified cyclodextrin;
[0010] Step A2: Add the modified cyclodextrin to deionized water, stir for 3-5 minutes at a speed of 60-80 r / min and a temperature of 40-50° C., remove the deionized water, cool to 0° C., add n-butyl lithium and tetrahydrofuran, react for 1-1.5 hours, add trifluoropropylmethylcyclotrisiloxane, heat to 20-25° C., react for 4-6 hours, add dimethylvinylchlorosilane, continue to react for 10-15 hours, adjust the pH value to neutral, and obtain a modified monomer.
[0011] Furthermore, the mass ratio of β-cyclodextrin, sodium hydroxide and sodium chloroacetate in step A1 is 4.5:4:8, and the molar ratio of the carboxyl group on carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane and dicyclohexylcarbodiimide is 1:1:1.2.
[0012] Furthermore, the amount ratio of the modified cyclodextrin, deionized water, n-butyl lithium, trifluoropropylmethylcyclotrisiloxane and dimethylvinylchlorosilane described in step A2 is 1 g: 5 mL: 20 mmol: 10 mmol.
[0013] Further, the modified additive is prepared by the following steps:
[0014] Step B1: Graphene oxide, ammonium tetrathiomolybdate and ethylene glycol are mixed evenly, reacted for 3-5 hours at a speed of 200-300 r / min and a temperature of 170-175° C., cooled to room temperature, filtered to remove the filtrate, dispersed the substrate in toluene, added 3-dimethylamino-1-propanol and p-toluenesulfonic acid, reacted for 4-6 hours at a speed of 120-150 r / min and a temperature of 110-120° C., and obtained pretreated graphene;
[0015] Step B2: Disperse the pretreated graphene in ethyl acetate, add ethyl bromide, and stir the reaction for 10-15 hours at a speed of 200-300 r / min and a temperature of 50-60°C to obtain modified graphene, mix N,N-dimethylhexadecyl-1-amine, propylene bromide and ethyl acetate, and stir the reaction for 10-15 hours at a speed of 200-300 r / min and a temperature of 50-60°C, add modified graphene and montmorillonite, raise the temperature to 80-85°C, and continue the reaction for 8-10 hours to obtain a modified additive.
[0016] Furthermore, the amount ratio of graphene oxide, ammonium tetrathiomolybdate and ethylene glycol described in step B1 is 1 mg:2 mg:1 mL, the amount ratio of substrate and 3-dimethylamino-1-propanol is 1 g:1 mL, and the amount of p-toluenesulfonic acid is 1% of the mass of 3-dimethylamino-1-propanol.
[0017] Furthermore, the amount ratio of the pretreated graphene and ethyl bromide in step B2 is 1g:1mL, and the amount ratio of N,N-dimethylhexadecyl-1-amine, propylene bromide, modified graphene and montmorillonite is 5mmo l:8mmo l:1g:5g.
[0018] The beneficial effects of the present invention are as follows: a drag reducer for fracturing prepared by the present invention is prepared by polymerization with modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and octadecyl methacrylate as raw materials; the modified monomer is reacted with beta-cyclodextrin and sodium chloroacetate as raw materials, so that the hydroxyl group on the beta-cyclodextrin reacts with the chlorine atom site on the sodium chloroacetate to prepare carboxymethyl cyclodextrin; the carboxymethyl cyclodextrin and (3-aminopropyl) dimethylethoxysilane are reacted, so that the carboxyl group on the carboxymethyl cyclodextrin and the amino group on the (3-aminopropyl) dimethylethoxysilane undergo a dehydration reaction to prepare the modified cyclodextrin; the modified cyclodextrin is added into water and stirred to convert the siloxane on the surface into silanol; the modified cyclodextrin is then ring-opening polymerized with trifluoropropylmethylcyclotrisiloxane; and finally, dimethylvinylchlorosilane is used for end-capping to form a double-bond-end-capped polysiloxane on the surface of the modified cyclodextrin molecule to prepare the modified monomer.
[0019] The modified additive uses graphene oxide and ammonium tetrathiomolybdate as raw materials, molybdenum disulfide is loaded on the graphene oxide, 3-dimethylamino-1-propanol and p-toluenesulfonic acid are added, so that the carboxyl group on the surface of the graphene oxide and the hydroxyl group on the 3-dimethylamino-1-propanol are esterified to obtain pretreated graphene, the pretreated graphene is treated with ethyl bromide, so that the bromine atom site on the ethyl bromide reacts with the dimethylamino group on the surface of the pretreated graphene to form a quaternary ammonium salt structure, N,N-dimethylhexadecyl-1-amine and propylene bromide react to form a quaternary ammonium salt structure containing a double bond, the modified graphene and montmorillonite are added, the modified graphene and montmorillonite are compounded through ion exchange, and the surface contains a double bond to obtain the modified additive.
[0020] The drag reducer molecule contains organic silicon segments, which can improve its own rigidity and thus increase the temperature resistance. The drag reducer can adhere to the pore surface during use. The organic silicon segments, long-chain alkyl and fluorocarbon structures make the drag reducer have a good hydrophobic effect, thereby forming a hydrophobic film on the surface. At the same time, it contains nano-inorganic substances that can effectively prevent the hydration and expansion of clay minerals in the formation, further reducing the resistance. The side chain contains cyclodextrin cavities, thereby increasing the sand carrying capacity of the fracturing fluid. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] A method for preparing a drag reducer for fracturing, comprising the following steps:
[0024] The modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, octadecyl methacrylate and DMF were mixed evenly, nitrogen was introduced for protection, potassium persulfate was added and stirred at a speed of 120 r / min and a temperature of 25°C, and the mixture was reacted for 4 hours to obtain a drag reducer for fracturing.
[0025] The dosage ratio of the modified monomer, the modified additive, acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and methacrylate octadecyl is 3 mol:50g:75 mol:20 mol:5 mol:0.04 mol, and the dosage of potassium persulfate is 0.05% of the total mass of the modified monomer, the modified additive, acrylamide, sodium p-styrene sulfonate, 2-acrylamide-2-methylpropanesulfonic acid and methacrylate octadecyl.
[0026] The modified monomer is prepared by the following steps:
[0027] Step A1: β-cyclodextrin, sodium hydroxide and deionized water are mixed, stirred and sodium chloroacetate is added at a speed of 120 r / min and a temperature of 25° C., and the reaction is carried out for 3 hours, and the pH value is adjusted to 5 to obtain carboxymethyl cyclodextrin; carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane, dicyclohexylcarbodiimide and toluene are mixed, and the reaction is carried out at a speed of 60 r / min and a temperature of 40° C. for 6 hours to obtain modified cyclodextrin;
[0028] Step A2: Add the modified cyclodextrin to deionized water, stir for 3 minutes at a speed of 60 r / min and a temperature of 40°C, remove the deionized water, cool to 0°C, add n-butyl lithium and tetrahydrofuran, react for 1 hour, add trifluoropropylmethylcyclotrisiloxane, heat to 20°C, react for 4 hours, add dimethylvinylchlorosilane, continue to react for 10 hours, adjust the pH value to neutral, and obtain a modified monomer.
[0029] The mass ratio of β-cyclodextrin, sodium hydroxide and sodium chloroacetate described in step A1 is 4.5:4:8, and the molar ratio of the carboxyl group on carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane and dicyclohexylcarbodiimide is 1:1:1.2.
[0030] The amount ratio of the modified cyclodextrin, deionized water, n-butyl lithium, trifluoropropylmethylcyclotrisiloxane and dimethylvinylchlorosilane described in step A2 is 1g:5mL:20mmo l:10mmo l.
[0031] The modified additive is prepared by the following steps:
[0032] Step B1: Graphene oxide, ammonium tetrathiomolybdate and ethylene glycol are mixed evenly, reacted at a speed of 200 r / min and a temperature of 170°C for 3 hours, then cooled to room temperature, filtered to remove the filtrate, dispersed the substrate in toluene, added 3-dimethylamino-1-propanol and p-toluenesulfonic acid, reacted at a speed of 120 r / min and a temperature of 110°C for 4 hours to obtain pretreated graphene;
[0033] Step B2: Disperse the pretreated graphene in ethyl acetate, add ethyl bromide, and stir the reaction for 10 hours at a speed of 200 r / min and a temperature of 50°C to obtain modified graphene; mix N,N-dimethylhexadecyl-1-amine, propylene bromide and ethyl acetate, and stir the reaction for 10 hours at a speed of 200 r / min and a temperature of 50°C; add modified graphene and montmorillonite, raise the temperature to 80°C, and continue the reaction for 8 hours to obtain a modified additive.
[0034] The amount ratio of graphene oxide, ammonium tetrathiomolybdate and ethylene glycol described in step B1 is 1 mg:2 mg:1 mL, the amount ratio of substrate and 3-dimethylamino-1-propanol is 1 g:1 mL, and the amount of p-toluenesulfonic acid is 1% of the mass of 3-dimethylamino-1-propanol.
[0035] The amount ratio of the pretreated graphene and ethyl bromide described in step B2 is 1g:1mL, and the amount ratio of N,N-dimethylhexadecyl-1-amine, propylene bromide, modified graphene and montmorillonite is 5mmo l:8mmo l:1g:5g.
[0036] Example 2
[0037] A method for preparing a drag reducer for fracturing, comprising the following steps:
[0038] The modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, octadecyl methacrylate and DMF were mixed evenly, nitrogen was introduced for protection, potassium persulfate was added and stirred at a speed of 120 r / min and a temperature of 28° C., and the mixture was reacted for 5 hours to obtain a drag reducer for fracturing.
[0039] The dosage ratio of the modified monomer, the modified additive, acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and methacrylate octadecyl is 3 mol:50g:75 mol:20 mol:5 mol:0.04 mol, and the dosage of potassium persulfate is 0.05% of the total mass of the modified monomer, the modified additive, acrylamide, sodium p-styrene sulfonate, 2-acrylamide-2-methylpropanesulfonic acid and methacrylate octadecyl.
[0040] The modified monomer is prepared by the following steps:
[0041] Step A1: β-cyclodextrin, sodium hydroxide and deionized water are mixed, stirred and sodium chloroacetate is added at a speed of 120 r / min and a temperature of 28° C., and the reaction is carried out for 4 hours, and the pH value is adjusted to 5 to obtain carboxymethyl cyclodextrin; carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane, dicyclohexylcarbodiimide and toluene are mixed, and the reaction is carried out at a speed of 60 r / min and a temperature of 45° C. for 7 hours to obtain modified cyclodextrin;
[0042] Step A2: Add the modified cyclodextrin to deionized water, stir for 4 min at a speed of 60 r / min and a temperature of 45°C, remove the deionized water, cool to 0°C, add n-butyl lithium and tetrahydrofuran, react for 1.3 h, add trifluoropropylmethylcyclotrisiloxane, raise the temperature to 23°C, react for 5 h, add dimethylvinylchlorosilane, continue to react for 13 h, adjust the pH value to neutral, and obtain a modified monomer.
[0043] The mass ratio of β-cyclodextrin, sodium hydroxide and sodium chloroacetate described in step A1 is 4.5:4:8, and the molar ratio of the carboxyl group on carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane and dicyclohexylcarbodiimide is 1:1:1.2.
[0044] The amount ratio of the modified cyclodextrin, deionized water, n-butyl lithium, trifluoropropylmethylcyclotrisiloxane and dimethylvinylchlorosilane described in step A2 is 1g:5mL:20mmo l:10mmo l.
[0045] The modified additive is prepared by the following steps:
[0046] Step B1: Graphene oxide, ammonium tetrathiomolybdate and ethylene glycol are mixed evenly, reacted at a speed of 300 r / min and a temperature of 170°C for 4 hours, then cooled to room temperature, filtered to remove the filtrate, dispersed the substrate in toluene, added 3-dimethylamino-1-propanol and p-toluenesulfonic acid, reacted at a speed of 120 r / min and a temperature of 115°C for 5 hours to obtain pretreated graphene;
[0047] Step B2: Disperse the pretreated graphene in ethyl acetate, add ethyl bromide, stir and react for 13 hours at a speed of 200 r / min and a temperature of 55°C to obtain modified graphene, mix N,N-dimethylhexadecyl-1-amine, propylene bromide and ethyl acetate, stir and react for 13 hours at a speed of 200 r / min and a temperature of 55°C, add modified graphene and montmorillonite, raise the temperature to 83°C, and continue to react for 9 hours to obtain a modified additive.
[0048] The amount ratio of graphene oxide, ammonium tetrathiomolybdate and ethylene glycol described in step B1 is 1 mg:2 mg:1 mL, the amount ratio of substrate and 3-dimethylamino-1-propanol is 1 g:1 mL, and the amount of p-toluenesulfonic acid is 1% of the mass of 3-dimethylamino-1-propanol.
[0049] The amount ratio of the pretreated graphene and ethyl bromide described in step B2 is 1g:1mL, and the amount ratio of N,N-dimethylhexadecyl-1-amine, propylene bromide, modified graphene and montmorillonite is 5mmo l:8mmo l:1g:5g.
[0050] Example 3
[0051] A method for preparing a drag reducer for fracturing, comprising the following steps:
[0052] The modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, octadecyl methacrylate and DMF were mixed evenly, nitrogen was introduced for protection, potassium persulfate was added and stirred at a speed of 150 r / min and a temperature of 30° C., and the mixture was reacted for 6 hours to obtain a drag reducer for fracturing.
[0053] The dosage ratio of the modified monomer, the modified additive, acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and methacrylate octadecyl is 3 mol:50g:75 mol:20 mol:5 mol:0.04 mol, and the dosage of potassium persulfate is 0.05% of the total mass of the modified monomer, the modified additive, acrylamide, sodium p-styrene sulfonate, 2-acrylamide-2-methylpropanesulfonic acid and methacrylate octadecyl.
[0054] The modified monomer is prepared by the following steps:
[0055] Step A1: β-cyclodextrin, sodium hydroxide and deionized water are mixed, stirred and sodium chloroacetate is added at a speed of 150 r / min and a temperature of 30° C., and the reaction is carried out for 5 hours, and the pH value is adjusted to 5 to obtain carboxymethyl cyclodextrin; carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane, dicyclohexylcarbodiimide and toluene are mixed, and the reaction is carried out at a speed of 80 r / min and a temperature of 50° C. for 8 hours to obtain modified cyclodextrin;
[0056] Step A2: Add the modified cyclodextrin to deionized water, stir for 5 minutes at a speed of 80 r / min and a temperature of 50°C, remove the deionized water, cool to 0°C, add n-butyl lithium and tetrahydrofuran, react for 1.5 hours, add trifluoropropyl methylcyclotrisiloxane, raise the temperature to 25°C, react for 6 hours, add dimethylvinyl chlorosilane, continue to react for 15 hours, adjust the pH value to neutral, and obtain a modified monomer.
[0057] The mass ratio of β-cyclodextrin, sodium hydroxide and sodium chloroacetate described in step A1 is 4.5:4:8, and the molar ratio of the carboxyl group on carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane and dicyclohexylcarbodiimide is 1:1:1.2.
[0058] The amount ratio of the modified cyclodextrin, deionized water, n-butyl lithium, trifluoropropylmethylcyclotrisiloxane and dimethylvinylchlorosilane described in step A2 is 1g:5mL:20mmo l:10mmo l.
[0059] The modified additive is prepared by the following steps:
[0060] Step B1: Graphene oxide, ammonium tetrathiomolybdate and ethylene glycol are mixed evenly, reacted at a speed of 300 r / min and a temperature of 175°C for 5 hours, cooled to room temperature, filtered to remove the filtrate, dispersed the substrate in toluene, added 3-dimethylamino-1-propanol and p-toluenesulfonic acid, reacted at a speed of 150 r / min and a temperature of 120°C for 6 hours to obtain pretreated graphene;
[0061] Step B2: Disperse the pretreated graphene in ethyl acetate, add ethyl bromide, stir and react for 15 hours at a speed of 300 r / min and a temperature of 60°C to obtain modified graphene, mix N,N-dimethylhexadecyl-1-amine, propylene bromide and ethyl acetate, stir and react for 15 hours at a speed of 300 r / min and a temperature of 60°C, add modified graphene and montmorillonite, raise the temperature to 85°C, and continue the reaction for 10 hours to obtain a modified additive.
[0062] The amount ratio of graphene oxide, ammonium tetrathiomolybdate and ethylene glycol described in step B1 is 1 mg:2 mg:1 mL, the amount ratio of substrate and 3-dimethylamino-1-propanol is 1 g:1 mL, and the amount of p-toluenesulfonic acid is 1% of the mass of 3-dimethylamino-1-propanol.
[0063] The amount ratio of the pretreated graphene and ethyl bromide described in step B2 is 1g:1mL, and the amount ratio of N,N-dimethylhexadecyl-1-amine, propylene bromide, modified graphene and montmorillonite is 5mmo l:8mmo l:1g:5g.
[0064] Comparative Example 1
[0065] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.
[0066] Comparative Example 2
[0067] Compared with Example 1, this comparative example uses hexamethylcyclotrisiloxane instead of trifluoropropylmethylcyclotrisiloxane, and the other steps are the same.
[0068] Comparative Example 3
[0069] Compared with Example 1, this comparative example uses trimethylsilanol instead of modified cyclodextrin, and the other steps are the same.
[0070] Comparative Example 4
[0071] Compared with Example 1, this comparative example did not add ammonium tetrathiomolybdate, and the remaining steps were the same.
[0072] Comparative Example 5
[0073] Compared with Example 1, this comparative example does not add modified graphene, and the remaining steps are the same.
[0074] Comparative Example 6
[0075] Compared with Example 1, no modifying additive was added in this comparative example, and the remaining steps were the same.
[0076] The drag reducers prepared in Examples 1-3 and Comparative Examples 1-6 were prepared into 0.05 wt% aqueous solutions at 25°C and added to a dissolution tank. The solutions were pumped out and entered the test section through a rotor flowmeter. The flow rate was measured by a rotor flowmeter, and the flow rate was controlled by a frequency converter to measure the pressure drop of the solution through the test section. The diameter of the test circular tube was 0.635 cm, the length of the test tube section was 3 meters, and the diameter was 10 mm. The drag reduction rate was measured at flow rates of 5 m / s, 10 m / s, 15 m / s and 20 m / s. The test results are shown in the following table.
[0077] 5m / s drag reduction rate 10m / s drag reduction rate 15m / s drag reduction rate 20m / s drag reduction rate Example 1 75.7 78.6 80.3 83.8 Example 2 75.9 79.1 80.6 84.1 Example 3 76.3 79.5 81.1 84.3 Comparative Example 1 53.8 54.3 55.4 56.1 Comparative Example 2 74.5 74.9 75.7 76.5 Comparative Example 3 72.6 73.2 74.4 75.1 Comparative Example 4 73.1 73.8 74.5 75.3 Comparative Example 5 70.6 71.7 72.9 73.3 Comparative Example 6 61.2 61.6 62.4 63.8
[0078] It can be seen from the above table that this application has a very good drag reduction effect.
[0079] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a drag reducer for fracturing, characterized in that: The specific steps include: The modified monomer, the modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, octadecyl methacrylate and DMF are uniformly mixed, nitrogen is introduced for protection, potassium persulfate is added for stirring, and a reaction is carried out to prepare a drag reducer for fracturing; The usage ratio of the modified monomer, modified additive, acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and octadecyl methacrylate is 3 mol:50 g:75 mol:20 mol:5 mol:0.04 mol; The modified monomer is prepared by the following steps: Step A1: β-cyclodextrin, sodium hydroxide and deionized water are mixed, stirred and sodium chloroacetate is added, and after reaction, the pH is adjusted to be acidic to obtain carboxymethyl cyclodextrin, and carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane, dicyclohexylcarbodiimide and toluene are mixed and reacted to obtain modified cyclodextrin; Step A2: adding the modified cyclodextrin to deionized water and stirring, removing the deionized water, cooling to 0°C, adding n-butyl lithium and tetrahydrofuran, reacting, adding trifluoropropylmethylcyclotrisiloxane, heating to react, adding dimethylvinylchlorosilane, continuing to react, adjusting the pH value to neutral, and obtaining a modified monomer; The modified additive is prepared by the following steps: Step B1: After graphene oxide, ammonium tetrathiomolybdate and ethylene glycol are mixed and reacted, the temperature is cooled to room temperature, the filtrate is filtered to remove the filtrate, the substrate is dispersed in toluene, 3-dimethylamino-1-propanol and p-toluenesulfonic acid are added, and the reaction is carried out to obtain pretreated graphene; Step B2: Disperse the pretreated graphene in ethyl acetate, add ethyl bromide, stir and react to obtain modified graphene, mix N,N-dimethylhexadecyl-1-amine, propylene bromide and ethyl acetate, stir and react, add modified graphene and montmorillonite, heat and continue to react to obtain a modified additive.
2. The method for preparing a drag reducer for fracturing according to claim 1, characterized in that: The mass ratio of β-cyclodextrin, sodium hydroxide and sodium chloroacetate in step A1 is 4.5:4:8, and the molar ratio of the carboxyl group on carboxymethyl cyclodextrin, (3-aminopropyl) dimethylethoxysilane and dicyclohexylcarbodiimide is 1:1:1.
2.
3. The method for preparing a drag reducer for fracturing according to claim 2, characterized in that: The amount ratio of the modified cyclodextrin, deionized water, n-butyl lithium, trifluoropropylmethylcyclotrisiloxane and dimethylvinylchlorosilane described in step A2 is 1 g: 5 mL: 20 mmol: 10 mmol.
4. The method for preparing a drag reducer for fracturing according to claim 1, characterized in that: The amount ratio of graphene oxide, ammonium tetrathiomolybdate and ethylene glycol described in step B1 is 1 mg:2 mg:1 mL, and the amount ratio of substrate and 3-dimethylamino-1-propanol is 1 g:1 mL.
5. The method for preparing a drag reducer for fracturing according to claim 4, characterized in that: The amount ratio of the pretreated graphene and ethyl bromide described in step B2 is 1g:1mL, and the amount ratio of N,N-dimethylhexadecyl-1-amine, propylene bromide, modified graphene and montmorillonite is 5mmol:8mmol:1g:5g.
6. A drag reducer for fracturing, characterized in that: Prepared according to any one of the preparation methods described in claims 1-5.
Citation Information
Patent Citations
Clean fracturing fluid thickening agent for oil well and preparation method thereof
CN116948107A
Degradable temporary plugging agent for oil and gas well fracturing and preparation method thereof
CN117126652A
Reverse Emulsion-based Slick Water Concentration System with Drag Reduction, Flow Back Enhancement and Clay Stabilization Functions
US20180112119A1
Ultra-high temperature organic cross-linked fracturing fluid system
US20230193117A1