A gradient cemented carbide and preparation method thereof

Through the preparation method of gradient cemented carbide, dewaxing pre-sintering and coating treatment combined with plasma thermal spraying and secondary sintering technology, the problem of hardness and toughness taking into account the inhibitor residue and moisture influence is solved, and the problem of cemented carbide materials is realized. A high-performance alloy that takes into account both surface hardness and wear resistance.

CN118621169BActive Publication Date: 2024-11-26CHONGYI ZHANGYUAN TUNGSTEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115025.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The differences in the surface and internal tissue of existing cemented carbide mold materials make it difficult to balance hardness and toughness, and the effects of inhibitor residues and moisture lead to low magnetic or decarbonization of cobalt.

Method used

The gradient carbide preparation method is adopted, and the mixture after ball milling and drying of the granulated granulated is pressed and molded, dewaxed and pre-sintered and coated. Combined with plasma thermal spraying and secondary sintering processes, the thickness and performance of the gradient layer are controlled.

Benefits of technology

A gradient carbide that takes into account both surface hardness and wear resistance is achieved, ensuring the overall toughness and performance of the product, and preventing the problems of carbon loss and low cobalt magnetism.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of powder metallurgy, and specifically relates to a gradient cemented carbide and a preparation method thereof. The pressed green body is first subjected to dewaxing and pre-sintering treatment, so that the forming agent in the green body can be removed, and the strength of the green body can be improved, so that the product performance and size are not affected during the subsequent surface treatment; and the green body after dewaxing and pre-sintering treatment is not completely shrunk, and the gaps between the powders are conducive to the attachment of the gradient additive during plasma thermal spraying and the diffusion of the gradient additive during secondary sintering, so as to control the thickness of the gradient layer, and finally achieve a smaller surface WC particle size and a larger internal WC particle size, taking into account the surface hardness and wear resistance, and having better overall toughness; during the attachment process of the gradient additive, the water component is excluded, which effectively prevents the water from causing the green body carbon to lose and cause the product cobalt magnetism to be low or even decarburized. The gradient layer hardness of the gradient cemented carbide of the present invention is 1300~1700HV3, the non-gradient layer hardness is 1200~1600HV3, and the gradient layer thickness is 1000~8000μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and specifically relates to a gradient cemented carbide and a preparation method thereof. Background Art

[0002] Cemented carbide refers to a composite material made of refractory metal carbides and bonding metals (cobalt, nickel, iron) by powder metallurgy. Cemented carbide is widely used in cutting tools, mold manufacturing, wear-resistant accessories and other fields. In some mold material application fields, cemented carbide materials with high hardness and high toughness are required, but in general, hardness and toughness are in a trade-off relationship. The emergence of gradient alloys is an important means to solve the above problems. Cemented carbides with different structures on the surface and inside are prepared by process to obtain functional layers with different properties, thereby achieving cemented carbide mold materials with hardness, toughness and wear resistance. In the prior art, the inhibitor mixture is applied to the surface of the pressed green body, and the actual residual amount of additives on the surface is uncontrollable, and the thickness of the gradient layer cannot be controlled. At the same time, the surface of the pressed green body is applied with an aqueous solution, which is also easy to cause low magnetism of the alloy cobalt or even decarburization. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a gradient cemented carbide and a preparation method thereof.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for preparing a gradient cemented carbide comprises the following steps:

[0006] S1, taking a bonding metal, an inhibitor, and WC powder as raw materials, and adding a molding agent, and obtaining a mixed material after ball milling and drying and granulation;

[0007] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-sintering, and then cooling to obtain a dewaxed pre-sintered green body;

[0008] S3, coating the surface of the dewaxed pre-sintered green body to obtain a coated green body, wherein the coating thickness is 0.01-0.1 mm;

[0009] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering, and then cooling to obtain a gradient cemented carbide.

[0010] As a preferred embodiment of the method for preparing a gradient cemented carbide according to the present invention, in the step S1, in the raw materials, the binder metal accounts for 2.0-32.0wt%, the inhibitor accounts for 0.5-0.8wt%, and the balance is WC powder.

[0011] As a preferred embodiment of the method for preparing a gradient cemented carbide according to the present invention, in said step S1, the forming agent accounts for 2.0-2.5wt% of the raw material mass.

[0012] As a preferred embodiment of the method for preparing a gradient cemented carbide according to the present invention, in the step S1, the average Fisher particle size of the WC powder is 0.8-1.2 μm.

[0013] As a preferred embodiment of the method for preparing a gradient cemented carbide described in the present invention, in step S1, the bonding metal is cobalt powder or a mixed powder of cobalt powder and nickel powder; the molding agent is paraffin or PEG; and the inhibitor is a carbide or oxide of one or more elements of Cr, V, Ta, Nb, Ti, and Mo.

[0014] As a preferred embodiment of the method for preparing a gradient cemented carbide according to the present invention, in said step S2, the pre-burning temperature is 800-1000°C, and the pre-burning time is 0.5-1.0h.

[0015] As a preferred embodiment of the method for preparing a gradient cemented carbide described in the present invention, in step S3, the gradient additive is a carbide or oxide of one or more elements of Cr, V, Ta, Nb, Ti, and Mo, and its average Fisher grain size is 0.6-1.0 μm.

[0016] As a preferred embodiment of the method for preparing a gradient cemented carbide according to the present invention, in step S3, the gradient additive is attached to the surface of the product or a designated area by a plasma thermal spraying process.

[0017] As a preferred embodiment of the method for preparing a gradient cemented carbide according to the present invention, in step S4, the sintering temperature is 1380-1430° C., and the sintering time is 0.5-0.8 h.

[0018] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0019] A gradient cemented carbide is prepared by adopting the above-mentioned method for preparing the gradient cemented carbide.

[0020] As a preferred embodiment of the gradient cemented carbide described in the present invention, the gradient layer hardness of the gradient cemented carbide is 1300~1700HV3, the non-gradient layer hardness is 1200~1600HV3, and the gradient layer thickness is 1000~8000μm.

[0021] The beneficial effects of the present invention are as follows:

[0022] The present invention proposes a gradient cemented carbide and a preparation method thereof. The pressed green body is first subjected to a dewaxing and pre-sintering treatment, so that the forming agent in the green body can be removed, and the green body strength can be improved, so that the product performance and size are not affected during the subsequent surface treatment; and the green body is not completely shrunk after the dewaxing and pre-sintering treatment, and the gaps between the powders are conducive to the attachment of the gradient additive during plasma thermal spraying and the diffusion of the gradient additive during secondary sintering, so as to control the thickness of the gradient layer, and finally achieve a smaller surface WC particle size and a larger internal WC particle size, taking into account both surface hardness and wear resistance, and having better overall toughness; during the attachment process of the gradient additive, the water component is excluded, effectively preventing water from causing the green body carbon to lose and causing the product cobalt magnetism to be low or even decarburized. The gradient layer hardness of the gradient cemented carbide of the present invention is 1300~1700HV3, the non-gradient layer hardness is 1200~1600HV3, and the gradient layer thickness is 1000~8000μm. DETAILED DESCRIPTION

[0023] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] According to one aspect of the present invention, the present invention provides the following technical solution:

[0025] A method for preparing a gradient cemented carbide comprises the following steps:

[0026] S1, taking a bonding metal, an inhibitor, and WC powder as raw materials, and adding a molding agent, and obtaining a mixed material after ball milling and drying and granulation;

[0027] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-sintering, and then cooling to obtain a dewaxed pre-sintered green body;

[0028] S3, coating the surface of the dewaxed pre-sintered green body to obtain a coated green body, wherein the coating thickness is 0.01-0.1 mm;

[0029] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering, and then cooling to obtain a gradient cemented carbide.

[0030] Preferably, in step S1, in the raw materials, the binder metal accounts for 2.0-32.0wt%, the inhibitor accounts for 0.5-0.8wt%, and the balance is WC powder.

[0031] Preferably, in step S1, the molding agent accounts for 2.0-2.5wt% of the raw material mass.

[0032] Preferably, in step S1, the average Fisher grain size of the WC powder is 0.8-1.2 μm.

[0033] Preferably, in step S1, the bonding metal is cobalt powder or a mixed powder of cobalt powder and nickel powder; the molding agent is paraffin or PEG; and the inhibitor is a carbide or oxide of one or more elements of Cr, V, Ta, Nb, Ti, and Mo.

[0034] Preferably, in step S2, the pre-firing temperature is 800-1000°C and the pre-firing time is 0.5-1.0h. The pre-firing treatment and temperature of the present invention can improve the green body strength, so that the product performance and size are not affected during the subsequent surface treatment.

[0035] Preferably, in step S3, the gradient additive is a carbide or oxide of one or more elements of Cr, V, Ta, Nb, Ti, and Mo, and its average Fisher grain size is 0.6-1.0 μm.

[0036] Preferably, in step S3, the gradient additive is attached to the surface of the product or a designated area by a plasma thermal spraying process. The plasma thermal spraying process can accurately control the thickness of the inhibitor coating and designate the gradient area, which is beneficial to the control of the thickness of the gradient layer;

[0037] Preferably, in step S4, the sintering temperature is 1380-1430°C, and the sintering time is 0.5-0.8h. The coating process is combined with the secondary sintering process to control the thickness of the gradient layer, and finally achieve a smaller surface WC particle size and a larger internal WC particle size, taking into account the surface hardness and wear resistance, and having good overall toughness.

[0038] According to another aspect of the present invention, the present invention provides the following technical solution:

[0039] A gradient cemented carbide is prepared by the above-mentioned method for preparing the gradient cemented carbide, wherein the gradient layer hardness of the gradient cemented carbide is 1300-1700 HV3, the non-gradient layer hardness is 1200-1600 HV3, and the gradient layer thickness is 1000-8000 μm.

[0040] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0041] Example 1

[0042] A method for preparing a gradient cemented carbide comprises the following steps:

[0043] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 10.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0044] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0045] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.02 mm;

[0046] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.8 h, and then cooling to obtain a gradient cemented carbide.

[0047] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1643 HV3, the hardness of the non-gradient layer is 1550 HV3, and the thickness of the gradient layer is 2139 μm.

[0048] Example 2

[0049] A method for preparing a gradient cemented carbide comprises the following steps:

[0050] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 20.0wt%, the inhibitor accounts for 1.0wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0051] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 800° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0052] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.02 mm;

[0053] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.8 h, and then cooling to obtain a gradient cemented carbide.

[0054] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1355 HV3, the hardness of the non-gradient layer is 1258 HV3, and the thickness of the gradient layer is 2250 μm.

[0055] Example 3

[0056] A method for preparing a gradient cemented carbide comprises the following steps:

[0057] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 15.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0058] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0059] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.02 mm;

[0060] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.8 h, and then cooling to obtain a gradient cemented carbide.

[0061] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1472 HV3, the hardness of the non-gradient layer is 1385 HV3, and the thickness of the gradient layer is 2187 μm.

[0062] Example 4

[0063] A method for preparing a gradient cemented carbide comprises the following steps:

[0064] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 10.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0065] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0066] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0067] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.8 h, and then cooling to obtain a gradient cemented carbide.

[0068] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1657 HV3, the hardness of the non-gradient layer is 1556 HV3, and the thickness of the gradient layer is 5045 μm.

[0069] Example 5

[0070] A method for preparing a gradient cemented carbide comprises the following steps:

[0071] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 20.0wt%, the inhibitor accounts for 1.0wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0072] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 800° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0073] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0074] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.8 h, and then cooling to obtain a gradient cemented carbide.

[0075] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1373 HV3, the hardness of the non-gradient layer is 1252 HV3, and the thickness of the gradient layer is 5160 μm.

[0076] Example 6

[0077] A method for preparing a gradient cemented carbide comprises the following steps:

[0078] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 15.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0079] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0080] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0081] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.8 h, and then cooling to obtain a gradient cemented carbide.

[0082] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1481 HV3, the hardness of the non-gradient layer is 1387 HV3, and the thickness of the gradient layer is 5090 μm.

[0083] Example 7

[0084] A method for preparing a gradient cemented carbide comprises the following steps:

[0085] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 10.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0086] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0087] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0088] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering, the sintering temperature is 1470°C, the sintering time is 0.8h, and then cooling to obtain a gradient cemented carbide.

[0089] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1656 HV3, the hardness of the non-gradient layer is 1551 HV3, and the thickness of the gradient layer is 6905 μm.

[0090] Example 8

[0091] A method for preparing a gradient cemented carbide comprises the following steps:

[0092] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 20.0wt%, the inhibitor accounts for 1.0wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0093] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 800° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0094] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0095] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering, the sintering temperature is 1470°C, the sintering time is 0.8h, and then cooling to obtain a gradient cemented carbide.

[0096] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1377 HV3, the hardness of the non-gradient layer is 1256 HV3, and the thickness of the gradient layer is 7142 μm.

[0097] Example 9

[0098] A method for preparing a gradient cemented carbide comprises the following steps:

[0099] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 15.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0100] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0101] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0102] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering, the sintering temperature is 1470°C, the sintering time is 0.8h, and then cooling to obtain a gradient cemented carbide.

[0103] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1483 HV3, the hardness of the non-gradient layer is 1384 HV3, and the thickness of the gradient layer is 7080 μm.

[0104] Example 10

[0105] A method for preparing a gradient cemented carbide comprises the following steps:

[0106] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 10.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0107] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0108] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.02 mm;

[0109] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.5 h, and then cooling to obtain a gradient cemented carbide.

[0110] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1634 HV3, the hardness of the non-gradient layer is 1541 HV3, and the thickness of the gradient layer is 1512 μm.

[0111] Embodiment 11

[0112] A method for preparing a gradient cemented carbide comprises the following steps:

[0113] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 20.0wt%, the inhibitor accounts for 1.0wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0114] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 800° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0115] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.02 mm;

[0116] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.5 h, and then cooling to obtain a gradient cemented carbide.

[0117] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1345 HV3, the hardness of the non-gradient layer is 1258 HV3, and the thickness of the gradient layer is 1630 μm.

[0118] Example 12

[0119] A method for preparing a gradient cemented carbide comprises the following steps:

[0120] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 15.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0121] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0122] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.02 mm;

[0123] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.5 h, and then cooling to obtain a gradient cemented carbide.

[0124] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1469 HV3, the hardness of the non-gradient layer is 1376 HV3, and the thickness of the gradient layer is 1559 μm.

[0125] Embodiment 13

[0126] A method for preparing a gradient cemented carbide comprises the following steps:

[0127] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 10.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0128] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0129] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0130] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.5 h, and then cooling to obtain a gradient cemented carbide.

[0131] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1640 HV3, the hardness of the non-gradient layer is 1543 HV3, and the thickness of the gradient layer is 2987 μm.

[0132] Embodiment 14

[0133] A method for preparing a gradient cemented carbide comprises the following steps:

[0134] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 20.0wt%, the inhibitor accounts for 1.0wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0135] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 800° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0136] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0137] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.5 h, and then cooling to obtain a gradient cemented carbide.

[0138] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1361 HV3, the hardness of the non-gradient layer is 1260 HV3, and the thickness of the gradient layer is 3056 μm.

[0139] Embodiment 15

[0140] A method for preparing a gradient cemented carbide comprises the following steps:

[0141] S1. Take a bonding metal, an inhibitor, and WC powder as raw materials, add a molding agent, and obtain a mixture after ball milling, drying and granulation; among the raw materials, the bonding metal accounts for 15.0wt%, the inhibitor accounts for 0.5wt%, and the balance is WC powder; the molding agent accounts for 2.0wt% of the raw material mass; the average Fisher particle size of the WC powder is 1.0μm; the bonding metal is cobalt powder; the molding agent is paraffin; and the inhibitor is chromium carbide.

[0142] S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning, the pre-burning temperature is 1000° C., and the pre-burning time is 0.5 h; then cooling to obtain a dewaxed pre-burned green body;

[0143] S3, attaching a gradient additive to the surface of the product by a plasma thermal spraying process to obtain a coated green body, wherein the gradient additive is chromium carbide, and its average Fisher particle size is 0.8 μm; and the coating thickness is 0.1 mm;

[0144] S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1430° C. for a sintering time of 0.5 h, and then cooling to obtain a gradient cemented carbide.

[0145] The hardness of the gradient layer of the gradient cemented carbide prepared in this embodiment is 1476 HV3, the hardness of the non-gradient layer is 1380 HV3, and the thickness of the gradient layer is 3011 μm.

[0146] Comparative Example 1

[0147] The difference from Example 1 is that dewaxing and pre-burning are not performed in step S2.

[0148] Since the comparative example has not been dewaxed and pre-burned, the green compact strength is low during step S3, and the high temperature of the plasma thermal spraying process destroys the green compact, so step S4 cannot be performed.

[0149] Comparative Example 2

[0150] The difference from Example 1 is that the pre-firing temperature in step S2 is 700°C.

[0151] In this comparative example, since the pre-sintering temperature in step S2 is 700° C., the alloying degree of the pressed green sheet is low, but it is better than that in comparative example 1. Only slight edge loss occurs at the edge of the pressed green sheet, which affects the appearance quality of the product and the product appearance is unqualified.

[0152] Comparative Example 3

[0153] The difference from Example 1 is that the pre-firing temperature in step S2 is 1100°C.

[0154] The pre-sintering temperature of this comparative example is too high, the alloying degree of the green compact is high, the green compact shrinkage is greater than that of the low-temperature pre-sintering, and the pores are less than those of the low-temperature pre-sintering. The reduction of pores is not conducive to the diffusion of gradient additives, and ultimately affects the thickness of the gradient layer.

[0155] The hardness of the gradient layer of the gradient cemented carbide prepared in this comparative example is 1648 HV3, the hardness of the non-gradient layer is 1558 HV3, and the thickness of the gradient layer is only 783 μm.

[0156] Comparative Example 4

[0157] The difference from Example 1 is that step S4 is not performed.

[0158] The alloy in this comparative example has not been subjected to high-temperature liquid phase sintering, has not been completely alloyed, and cannot meet the use requirements.

[0159] Comparative Example 5

[0160] The difference from Example 1 is that the sintering temperature in step S4 is 1300°C.

[0161] The alloy of this comparative example did not reach the liquidus temperature of the bonding phase, was not fully alloyed, had many pores and holes, and could not meet the use requirements.

[0162] It can be seen from the above embodiments and comparative examples that the present invention first dewaxes and pre-sinters the pressed green body, which can remove the forming agent in the green body and improve the strength of the green body, so that the product performance and size are not affected during the subsequent surface treatment; and the green body after dewaxing and pre-sintering is not completely shrunk, and the gaps between the powders are conducive to the attachment of the gradient additive during plasma thermal spraying and the diffusion of the gradient additive during secondary sintering, so as to control the thickness of the gradient layer, and finally achieve a smaller surface WC particle size and a larger internal WC particle size, taking into account the surface hardness and wear resistance, and having better overall toughness; during the attachment process of the gradient additive, the water component is excluded, which effectively prevents water from causing the green body carbon to lose and cause the product cobalt magnetism to be low or even decarburized. The gradient layer hardness of the gradient cemented carbide of the present invention is 1300~1700HV3, the non-gradient layer hardness is 1200~1600HV3, and the gradient layer thickness is 1000~8000μm.

[0163] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a gradient cemented carbide, characterized in that: The steps include: S1, taking a bonding metal, an inhibitor, and WC powder as raw materials, and adding a molding agent, and obtaining a mixed material after ball milling and drying and granulation; S2, pressing the mixture to obtain a green body, placing the green body into a vacuum dewaxing furnace for pre-burning at a temperature of 800-1000° C., and then cooling to obtain a dewaxed pre-burned green body; S3, coating the surface of the dewaxed pre-sintered green body to obtain a coated green body, the coating thickness of which is 0.01-0.1 mm; the coating is to attach a gradient additive to the surface of the green body by a plasma thermal spraying process; S4, placing the coated green body into a vacuum sintering furnace for secondary sintering at a sintering temperature of 1380-1430°C, and then cooling to obtain a gradient cemented carbide.

2. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: Among the raw materials, the binder metal accounts for 2.0~32.0wt%, the inhibitor accounts for 0.5~0.8wt%, and the balance is WC powder.

3. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: In the step S1, the molding agent accounts for 2.0-2.5wt% of the raw material mass.

4. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: In the step S1, the average Fisher grain size of the WC powder is 0.8-1.2 μm.

5. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: In step S1, the bonding metal is cobalt powder or a mixed powder of cobalt powder and nickel powder; the molding agent is paraffin or PEG; and the inhibitor is a carbide or oxide of one or more elements of Cr, V, Ta, Nb, Ti, and Mo.

6. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: In the step S2, the pre-burning time is 0.5-1.0h.

7. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: In step S3, the gradient additive is a carbide or oxide of one or more elements of Cr, V, Ta, Nb, Ti, and Mo, and its average Fisher grain size is 0.6-1.0 μm.

8. The method for preparing a gradient cemented carbide according to claim 1, characterized in that: In step S4, the sintering time is 0.5-0.8h.

9. A gradient cemented carbide prepared by the method for preparing a gradient cemented carbide according to any one of claims 1 to 8, wherein the gradient layer hardness of the gradient cemented carbide is 1300-1700 HV3, the non-gradient layer hardness is 1200-1600 HV3, and the gradient layer thickness is 1000-8000 μm.