A kind of cemented carbide and preparation method thereof
By adding nanotungsten powder to cemented carbide and adopting a specific sintering process, the quality stability of cemented carbide is solved when improving hardness and toughness, and high performance cemented carbide preparation is achieved, with high hardness and high toughness and strength characteristics, and simplify the process flow, suitable for industrial production.
Patent Information
- Application Number
- CN202411115060.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-14
AI Technical Summary
When existing cemented carbides improve hardness and toughness, they are prone to problems such as oxidation, decarbonization, carburization, uneven dispersion and abnormal grain growth, resulting in unstable product quality. Commonly used ceramic additives and high-priced metals such as Ru /Re is difficult to accept.
The carbon content is controlled by adding nanotungsten powder, combined with the ingredients and ball milling of powders such as WC, Co, Cr3C2, VC, etc., and molding is used to sinter it in a vacuum pressure sintering furnace to control the sintering temperature and pressure to prepare high-performance carbide .
The high hardness, high toughness and high strength of cemented carbides are achieved, with a density of ≥14.75g/cm3, hardness of ≥2150HV, cracking toughness KIC of 7.7~8.1MPa·m1/2, bending strength of ≥2500MPa, and the process flow is simple and practical , easy to implement industrially.
Smart Images

Figure CN118621173B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of powder metallurgy, and specifically relates to a cemented carbide and a preparation method thereof. More specifically, the present invention relates to a method for preparing high-performance cemented carbide by controlling the carbon content by adding nano-tungsten powder. Background Art
[0002] Cemented carbide is a composite material made of hard phases such as WC, TiC, NbC, TaC and bonding phases such as Co, Ni and Fe, prepared by powder metallurgy. It has high hardness, high wear resistance and high strength and is widely used in cutting tools, mining, wear-resistant parts and tooling. However, due to the trade-off between hardness and toughness, in order to improve hardness, toughness and strength at the same time, by adopting the methods of fine grain strengthening and solid solution strengthening, compared with conventional grain WC-Co alloy materials, low cobalt (≤6wt%Co) ultrafine grains have higher comprehensive mechanical properties such as hardness, strength and wear resistance, and have always been a research hotspot in high-end applications such as precision information industry, high-speed cutting, micro-engraving and military weapons. This type of alloy has a WC grain size of 0.3~0.5μm, WC powder is very fine, has a large specific surface area, and has a low cobalt content. The carbon range of the two-phase region is very narrow. If the industrial production process is not properly controlled, it is very easy to experience oxidation, decarburization, carburization, uneven dispersion and abnormal grain growth, resulting in unstable product quality and ultimately affecting product performance. For this reason, high-performance, low-cobalt ultrafine-grained cemented carbide has been developed, which has huge market prospects and outstanding economic benefits.
[0003] At present, the main methods to improve the strength and toughness of WC cemented carbide are: introducing ceramic additives, refining WC grains, and strengthening the bonding phase. In recent years, there have been many studies on the methods of strengthening with ceramic additives. Commonly used ceramic additives are metal carbides, oxides, borides and nitrides, and different ceramic additives show different strengthening and toughening mechanisms. However, ceramic additives are hard and brittle in nature and are not easy to add too much. Secondly, the method of refining the WC grain size usually uses ultrafine (0.3~0.5μm) or nano WC powder. Although it can significantly improve the comprehensive mechanical properties of the alloy, it is easy to cause agglomeration, uneven dispersion, oxidation, grain growth and other quality problems due to the powder being too fine, and it is not easy to control mass production; strengthening the bonding phase refers to improving the strength of the cobalt phase by regulating the phase composition and structure of the cobalt phase. It is usually done by adding metals such as Ru / Re or changing the cobalt phase fcc to hcp phase to improve the strength of the cobalt phase. However, the price of Ru / Re metal is high, and the market cannot accept the high raw material cost. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a cemented carbide and a preparation method thereof.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A method for preparing cemented carbide comprises the following steps:
[0007] S1, 90.89-97.2wt% of WC powder, 2-6wt% of cobalt powder, 0.2-0.8wt% of Cr3C2 powder, 0.2-0.6wt% of VC powder and 0.4-1.71wt% of nano tungsten powder are mixed to obtain a mixture, and the mixture is ball-milled, dried and sieved;
[0008] S2. The dried and sieved mixture is sintered in a vacuum pressure sintering furnace by compression molding to obtain a cemented carbide.
[0009] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in step S1, the total carbon content of the WC powder is 6.10-6.14 wt %, and the specific surface area BET is 2.2-2.6 m 2 / g; the particle size of cobalt powder is <1μm.
[0010] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in step S1, the BET specific surface area of the nano tungsten powder is 3.0-7.5 m 2 / g.
[0011] As a preferred embodiment of the method for preparing cemented carbide described in the present invention, in step S1, the nano tungsten powder is mixed with 0.5-1.0wt% paraffin wax to form agglomerated powder with an average particle size of 30-80μm.
[0012] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in said step S1, the mass of the forming agent added during ball milling is 2-2.5wt% of the mass of the mixture.
[0013] As a preferred embodiment of the method for preparing cemented carbide described in the present invention, wherein: in the step S1, the mass of the dispersant added during ball milling is 0.2-1.0wt% of the mass of the mixture, and the dispersant is at least one of lauryl alcohol, stearyl alcohol, polysorbate, and polyethylene glycol.
[0014] As a preferred embodiment of the method for preparing cemented carbide described in the present invention, wherein: in the step S1, the ball milling medium is anhydrous ethanol, and the liquid-solid ratio of anhydrous ethanol and the mixture is controlled to be (3~3.5)mL:1g; the ball milling speed is 250~300r / min, the ball-to-material ratio is (4~8):1, and the ball milling time is 8~14h.
[0015] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in step S1, the drying temperature is 85-120° C. and the drying time is 20-50 min.
[0016] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in the step S1, a 60-mesh screen is used for screening.
[0017] As a preferred embodiment of the method for preparing cemented carbide described in the present invention, in step S2, the sintering process is as follows: the sintering temperature is 1380-1430°C, the sintering pressure is 4.0-9.0 MPa, and the sintering time is 30-90 min.
[0018] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:
[0019] A cemented carbide is prepared by adopting the above-mentioned method for preparing the cemented carbide.
[0020] As a preferred embodiment of the cemented carbide of the present invention, the density of the cemented carbide is ≥14.75 g / cm 3 , hardness ≥ 2150HV, crack toughness KIC 7.7~8.1MPa·m 1 / 2 ; Bending strength ≥ 2500MPa; In the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0021] The beneficial effects of the present invention are as follows:
[0022] The present invention provides a cemented carbide and a preparation method thereof. By adding nano tungsten powder to control the carbon content, the cemented carbide prepared by the method can simultaneously obtain high hardness, high toughness and high strength. The method has the characteristics of simple and practical process flow, strong operability and easy industrial implementation. The density of the cemented carbide prepared by the present invention is ≥14.75g / cm 3 , hardness ≥ 2150HV, crack toughness KIC 7.7~8.1MPa·m 1 / 2 ; Bending strength ≥ 2500MPa; In the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0024] Figure 1 This is a picture of the cemented carbide prepared in Example 1 of the present invention.
[0025] Figure 2 This is a picture of the cemented carbide prepared in Comparative Example 1 of the present invention.
[0026] Figure 3 This is a picture of the cemented carbide prepared in Comparative Example 2 of the present invention.
[0027] Figure 4 This is a picture of the cemented carbide prepared in Comparative Example 3 of the present invention.
[0028] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0029] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] According to one aspect of the present invention, the present invention provides the following technical solution:
[0031] A method for preparing cemented carbide comprises the following steps:
[0032] S1, 90.89-97.2wt% of WC powder, 2-6wt% of cobalt powder, 0.2-0.8wt% of Cr3C2 powder, 0.2-0.6wt% of VC powder and 0.4-1.71wt% of nano tungsten powder are mixed to obtain a mixture, and the mixture is ball-milled, dried and sieved;
[0033] S2. The dried and sieved mixture is sintered in a vacuum pressure sintering furnace by compression molding to obtain a cemented carbide.
[0034] Preferably, in step S1, the total carbon content of the WC powder is 6.10-6.14 wt %, and the specific surface area BET is 2.2-2.6 m 2 / g; the particle size of cobalt powder is <1μm.
[0035] Preferably, in step S1, the BET specific surface area of the nano tungsten powder is 3.0-7.5 m 2 / g. Nano tungsten powder has a very fine particle size and cannot be characterized by conventional FSSS particle size. The present invention uses specific surface area BET to characterize the particle size of tungsten powder. The specific surface area BET of nano tungsten powder is greater than 7.5 m 2 / g, the tungsten powder is extremely fine, and it starts to oxidize when it comes into contact with air, which is very easy to burn, posing a major safety hazard, and production control is very difficult. In addition, it is very easy to agglomerate, destroying the dispersion of tungsten, resulting in uneven organizational structure, uneven performance, and unstable use. The specific surface area of nano tungsten powder is less than 3.0 m 2 / g, the particle size is coarse, usually fsss is greater than or equal to 0.4μm, tungsten powder is too coarse, and the dispersion is prone to unevenness. For ultrafine grain grades, the particle size of tungsten carbide WC is 0.3~0.5μm, and the sintering temperature is usually low. Tungsten powder that is too coarse is difficult to dissolve in the bonding phase, and the solid solution strengthening effect is limited, which reduces the strength of the alloy.
[0036] Preferably, in step S1, since the nano tungsten powder is oxidized or even burned due to contact with the atmosphere, the nano tungsten powder of the present invention is preferably prepared by adding 0.5-1.0wt% of paraffin wax to granulate into agglomerated powder with an average particle size of 30-80μm. The added paraffin wax can form a film on the surface of the tungsten powder, wrap the tungsten powder, isolate the air and prevent oxidation. At the same time, the agglomerated tungsten powder has better fluidity than the nano powder, is easy to disperse by ball milling, and is more uniform.
[0037] Preferably, in step S1, the mass of the molding agent added during ball milling is 2-2.5wt% of the mass of the mixture, and the molding agent is paraffin.
[0038] Preferably, in step S1, the mass of the dispersant added during ball milling is 0.2-1.0 wt % of the mass of the mixture, and the dispersant is at least one of lauryl alcohol, stearyl alcohol, polysorbate, and polyethylene glycol.
[0039] Preferably, in step S1, the ball milling medium is anhydrous ethanol, and the liquid-solid ratio of anhydrous ethanol to the mixed material is controlled to be (3-3.5) mL:1 g; the ball milling speed is 250-300 r / min, the ball-to-material ratio is (4-8):1, and the ball milling time is 8-14 h.
[0040] Preferably, in step S1, the drying temperature is 85-120° C., and the drying time is 20-50 min.
[0041] Preferably, in step S1, a 60-mesh sieve is used for sieving.
[0042] Preferably, in step S2, the sintering process is: the sintering temperature is 1380-1430° C., the sintering pressure is 4.0-9.0 MPa, and the sintering time is 30-90 min.
[0043] According to another aspect of the present invention, the present invention provides the following technical solution:
[0044] A cemented carbide prepared by the above-mentioned method for preparing cemented carbide, wherein the density of the cemented carbide is ≥14.75 g / cm 3 , hardness ≥ 2150HV, crack toughness KIC 7.7~8.1MPa·m 1 / 2 ; Bending strength ≥ 2500MPa; In the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0045] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0046] Example 1
[0047] A method for preparing cemented carbide comprises the following steps:
[0048] S1. 91.49 g of WC powder, 6.0 g of cobalt powder, 0.6 g of Cr3C2 powder, 0.2 g of VC powder and 1.71 g of nano-tungsten powder were mixed to obtain a mixture, which was ball-milled and dried and sieved; the total carbon content of the WC powder was 6.11 wt%, and the specific surface area BET was 2.41 m 2 / g; the particle size of cobalt powder is <1μm; the specific surface area of nano tungsten powder is 3.5 m 2 / g; the mass of the molding agent added during ball milling is 2.2wt% of the mass of the mixture; the mass of the dispersant added during ball milling is 1wt% of the mass of the mixture, and the dispersant is lauryl alcohol; the medium for ball milling is anhydrous ethanol, and the liquid-solid ratio of anhydrous ethanol and the mixture is controlled to be 3.5)L:1g; the ball milling speed is 300r / min, the ball-to-material ratio is 6:1, and the ball milling time is 10h; the drying temperature is 95℃, and the drying time is 30min; a 60-mesh screen is used for screening.
[0049] S2. The dried and sieved mixture is sintered in a vacuum pressure sintering furnace by compression molding. The sintering process is as follows: sintering temperature is 1410° C., sintering pressure is 9.0 MPa, and sintering time is 60 min; and a cemented carbide is obtained.
[0050] The picture of the cemented carbide obtained in this embodiment is as follows Figure 1 As shown, its density is 14.79g / cm 3 , hardness is 2247HV, crack toughness KIC is 7.94MPa·m 1 / 2; The flexural strength is 2740MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0051] Example 2
[0052] The difference from Example 1 is that in step S1, 92.15 g of WC powder, 6.0 g of cobalt powder, 0.6 g of Cr3C2 powder, 0.2 g of VC powder and 1.05 g of nano tungsten powder are mixed to obtain a mixture.
[0053] The density of the cemented carbide obtained in this example is 14.76 g / cm 3 , hardness is 2245HV, crack toughness KIC is 7.71MPa·m 1 / 2 ; The flexural strength is 2539MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0054] Example 3
[0055] The difference from Example 1 is that in step S1, 92.80 g of WC powder, 6.0 g of cobalt powder, 0.6 g of Cr3C2 powder, 0.2 g of VC powder and 0.4 g of nano tungsten powder are mixed to obtain a mixture.
[0056] The density of the cemented carbide obtained in this example is 14.77 g / cm 3 , hardness is 2156HV, crack toughness KIC is 7.87MPa·m 1 / 2 ; The flexural strength is 2509MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0057] Example 4
[0058] The difference from Example 1 is that the BET specific surface area of the nano tungsten powder in step S1 is 4.1 m 2 / g, the nano tungsten powder is prepared by adding 0.8wt% of paraffin wax to the powder to form agglomerated powder with an average particle size of 50μm.
[0059] The density of the cemented carbide obtained in this example is 14.80 g / cm 3 , hardness is 2251HV, crack toughness KIC is 7.91MPa·m 1 / 2 ; The flexural strength is 2731MPa; in the metallographic microstructure, the porosity is A02B00, the non-combined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0060] Example 5
[0061] The difference from Example 4 is that the BET specific surface area of the nano tungsten powder in step S1 is 7.2 m 2 / g.
[0062] The density of the cemented carbide obtained in this example is 14.84 g / cm 3 , hardness is 2255HV, crack toughness KIC is 7.88MPa·m 1 / 2 ; The flexural strength is 2745MPa; in the metallographic microstructure, the porosity is A02B00, the non-combined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0063] Example 6
[0064] The difference from Example 4 is that the specific surface area of the nano tungsten powder in step S1 is 5.2 m 2 / g.
[0065] The density of the cemented carbide obtained in this example is 14.85 g / cm 3 , hardness is 2247HV, crack toughness KIC is 7.86MPa·m 1 / 2 ; The flexural strength is 2756MPa; in the metallographic microstructure, the porosity is A02B00, the non-combined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0066] Example 7
[0067] The difference from Example 1 is that the mass of the dispersant added during ball milling in step S1 is 0.4 wt % of the mass of the mixture, and the dispersant is stearyl alcohol.
[0068] The density of the cemented carbide obtained in this example is 14.78 g / cm 3 , hardness is 2234HV, crack toughness KIC is 7.99MPa·m 1 / 2 ; The flexural strength is 2743MPa; in the metallographic microstructure, the porosity is A02B00, the non-combined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0069] Example 8
[0070] The difference from Example 1 is that the mass of the dispersant added during ball milling in step S1 is 0.8 wt % of the mass of the mixture, and the dispersant is polyethylene glycol.
[0071] The density of the cemented carbide obtained in this example is 14.77 g / cm 3 , hardness is 2244HV, crack toughness KIC is 8.01MPa·m 1 / 2; The flexural strength is 2746MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0072] Comparative Example 1
[0073] The difference from Example 1 is that in step S1, 90.83 g of WC powder, 6.0 g of cobalt powder, 0.6 g of Cr3C2 powder, 0.2 g of VC powder and 2.37 g of nano tungsten powder are mixed to obtain a mixture.
[0074] The picture of the cemented carbide obtained in this comparative example is as follows Figure 2 As shown, its density is 14.81g / cm 3 , hardness is 2248HV, crack toughness KIC is 7.44MPa·m 1 / 2 ; The flexural strength is 1616MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, and the decarburized phase is E04.
[0075] Comparative Example 2
[0076] The difference from Example 1 is that in step S1, 93.17 g of WC powder, 6.0 g of cobalt powder, 0.6 g of Cr3C2 powder, 0.2 g of VC powder and 0.03 g of nano tungsten powder are mixed to obtain a mixture.
[0077] The picture of the cemented carbide obtained in this comparative example is as follows Figure 3 As shown, its density is 14.74g / cm 3 , hardness is 2096HV, crack toughness KIC is 7.38MPa·m 1 / 2 ; The flexural strength is 2157MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C04, and the decarburized phase is E00.
[0078] Comparative Example 3
[0079] The difference from Example 1 is that in step S1, 93.2 g of WC powder, 6.0 g of cobalt powder, 0.6 g of Cr3C2 powder, and 0.2 g of VC powder are mixed to obtain a mixture.
[0080] The picture of the cemented carbide obtained in this comparative example is as follows Figure 4 As shown, its density is 14.69g / cm 3 , hardness is 2065HV, crack toughness KIC is 7.28MPa·m 1 / 2 ; The flexural strength is 1999MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C06, and the decarburized phase is E00.
[0081] Comparative Example 4
[0082] The difference from Example 1 is that the specific surface area of the nano tungsten powder in step S1 is 2.2 m 2 / g.
[0083] The density of the cemented carbide obtained in this comparative example is 14.82 g / cm 3 , hardness is 2189HV, crack toughness KIC is 7.15MPa·m 1 / 2 ; The flexural strength is 2145MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there are 1 to 2 coarse grains of 3 to 6μm.
[0084] Comparative Example 5
[0085] The difference from Example 1 is that the specific surface area of the nano tungsten powder in step S1 is 8.0 m 2 / g.
[0086] The density of the cemented carbide obtained in this comparative example is 14.78 g / cm 3 , hardness is 2178HV, crack toughness KIC is 7.11MPa·m 1 / 2 ; The flexural strength is 2424MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there are 2 to 3 coarse grains of 3 to 6μm.
[0087] Comparative Example 6
[0088] The difference from Example 1 is that no dispersant is added in step S1.
[0089] The density of the cemented carbide obtained in this comparative example is 14.79 g / cm 3 , hardness is 2177HV, crack toughness KIC is 7.54MPa·m 1 / 2 ; The flexural strength is 2468MPa; in the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there are 2 coarse grains of 3~6μm.
[0090] It can be seen from the above examples and comparative examples that the present invention controls the carbon content by adding nano tungsten powder. The cemented carbide prepared by this method can simultaneously obtain high hardness, high toughness and high strength. The method has the characteristics of simple and practical process flow, strong operability and easy industrial implementation. The density of the cemented carbide prepared by the present invention is ≥14.75g / cm 3 , hardness ≥ 2150HV, crack toughness KIC 7.7~8.1MPa·m 1 / 2; Bending strength ≥ 2500MPa; In the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
[0091] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a cemented carbide, It is characterized in that The steps include: S1, 90.89~97.2wt% WC powder, 2~6wt% cobalt powder, 0.2~0.8wt% Cr 3 C 2 The mixture is prepared by mixing 0.2-0.6wt% VC powder and 0.4-1.71wt% nano tungsten powder, and then ball-milling the mixture and drying and sieving it. The total carbon content of the WC powder is 6.10-6.14wt%, and the specific surface area BET is 2.2-2.6m 2 / g; the particle size of cobalt powder is <1μm; the specific surface area of nano tungsten powder is 3.0~7.5m 2 / g, the nano tungsten powder is prepared by adding 0.5~1.0wt% of paraffin wax to form agglomerated powder with an average particle size of 30~80μm; S2. The dried and sieved mixture is sintered in a vacuum pressure sintering furnace by compression molding to obtain a cemented carbide having a density of ≥14.75 g / cm 3 , hardness ≥ 2150HV, crack toughness KIC 7.7~8.1MPa·m 1 / 2 ; Bending strength ≥ 2500MPa; In the metallographic microstructure, the porosity is A02B00, the uncombined carbon structure is C00, the decarburized phase is E00, and there is no coarse inclusion.
2. The method for preparing the cemented carbide according to claim 1, It is characterized in that In the step S1, the mass of the forming agent added during ball milling is 2-2.5wt% of the mass of the mixed material.
3. The method for preparing the cemented carbide according to claim 1, It is characterized in that In the step S1, the mass of the dispersant added during ball milling is 0.2-1.0wt% of the mass of the mixture, and the dispersant is at least one of lauryl alcohol, stearyl alcohol, polysorbate, and polyethylene glycol.
4. The method for preparing the cemented carbide according to claim 1, It is characterized in that In the step S1, the ball milling medium is anhydrous ethanol, and the liquid-solid ratio of anhydrous ethanol to the mixed material is controlled to be (3-3.5) mL:1 g; the ball milling speed is 250-300 r / min, the ball-to-material ratio is (4-8):1, and the ball milling time is 8-14 h.
5. The method for preparing the cemented carbide according to claim 1, It is characterized in that In the step S1, the drying temperature is 85-120° C., the drying time is 20-50 min, and a 60-mesh sieve is used for sieving.
6. The method for preparing the cemented carbide according to claim 1, It is characterized in that In step S2, the sintering process is as follows: the sintering temperature is 1380-1430° C., the sintering pressure is 4.0-9.0 MPa, and the sintering time is 30-90 min.
7. A cemented carbide, It is characterized in that The hard alloy is prepared by the preparation method of the hard alloy according to any one of claims 1 to 6.