A method for preparing anion exchange resin film and its application in extracting polysaccharides

By preparing anion exchange resin films with quaternary ammonium cation side chains and urea side chains, the problems of high energy consumption and resource waste in polysaccharide extraction in existing technologies have been solved, and efficient separation of sodium alginate and fucoidan has been achieved, improving product purity and resource utilization.

CN118638332BActive Publication Date: 2024-11-05YANTAI TAYHO ADVANCED MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095374.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-05
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Existing technologies that can only extract one type of polysaccharide or multiple types of polysaccharides at the same time are energy-intensive and require a large amount of organic solvents, resulting in low utilization of seaweed resources and environmental pollution problems.

Method used

An anion exchange resin membrane preparation method was adopted. By preparing a resin membrane with quaternary ammonium cation side chains and urea side chains, the specific adsorption of fucoidan on the membrane was utilized. Combined with treatment with a small amount of NaOH and ethanol, the efficient separation and extraction of sodium alginate and fucoidan were achieved.

Benefits of technology

It improves the purity and spinnability of sodium alginate products, reduces the content of fucoidan, lowers extraction costs, and achieves efficient separation of polysaccharides and recycling of resources, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638332B_ABST
    Figure CN118638332B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of biomass polysaccharide extraction, and specifically to a method for preparing an anion exchange resin film and its application in extracting polysaccharides. The method for preparing the anion exchange resin film is as follows: 1,6-diiodohexane and trimethylamine react in a solvent system to obtain a small molecule A; then react with N,N,N',N'-tetramethyl-1,6-hexanediamine to obtain a quaternary ammonium salt small molecule B, react PPO bromide with NaN3, add the quaternary ammonium salt small molecule B to react to obtain a product C, react product C with PPh3, and then react with isocyanate to obtain a product D, and separate and coat the product D, and dry it to obtain an anion exchange resin film. The anion exchange resin film is applied in a method for simultaneously extracting sodium alginate and fucoidan from seaweed, solving the problem that only one polysaccharide or multiple polysaccharides can be extracted simultaneously in the traditional extraction method, and the process energy consumption and the need to consume a large amount of solvent are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an anion exchange resin film and application thereof in extracting polysaccharides, belonging to the technical field of biomass polysaccharide extraction. Background Art

[0002] For many years, the development of seaweed at home and abroad, especially in my country, has always been the "old three" of iodine, alginic acid and mannitol. The industry as a whole is in a state of low grade, low level, low added value and low efficiency, and the market competitiveness of products and enterprises is weak. Therefore, the development of seaweed processing technology routes with high comprehensive utilization rate of seaweed resources, high added value of products and high process technology level is the current primary issue for industry workers.

[0003] Fucoidan and alginate are brown algae polysaccharides existing between and within brown algae cells. They are natural biomacromolecules with extremely high edible and medicinal value. At present, the extraction methods of alginate include acidification-acid coagulation, calcification-acid coagulation, calcification-ion exchange, enzymatic hydrolysis, ultrafiltration, etc.; the extraction methods of fucoidan include water extraction, acid extraction, alkali extraction, calcium chloride method, enzymatic hydrolysis, ultrafiltration, etc. These extraction methods can only extract one of the above two polysaccharides, and the other polysaccharide is often discharged along with industrial waste, which not only wastes a large amount of seaweed resources, but also brings a series of environmental pollution problems.

[0004] Chinese patent CN106008730B discloses a method for extracting fucoidan and alginic acid at the same time, firstly, a composite enzyme is used to enzymolyze kelp, and after solid-liquid separation, a calcium chloride solution is added to the diluted supernatant to obtain a calcium alginate hydrogel, and an excess of sodium carbonate is added to the remaining supernatant and alcohol precipitation is performed to obtain a crude fucoidan product. The extraction method is simple and effective, but there are the following two problems: first, the calcium salt of fucoidan is easily soluble in water, and the water content of the calcium alginate hydrogel is above 85%. Even if there is a subsequent washing and drying process, the alginate obtained in the end is also mixed with fucoidan, and the product purity is poor. In addition, the subsequent process of extracting fucoidan requires concentrating the clear liquid, otherwise a large amount of ethanol will be consumed for alcohol precipitation of fucoidan, and concentrating the clear liquid is very energy-consuming and has poor economic benefits.

[0005] Chinese patent application CN106957374A discloses a method for extracting fucoidan and alginate from algae, firstly freezing the shredded kelp, then adding a lysis-promoting agent to soak, adding ethanol to different ethanol concentrations to the supernatant after filtration, collecting the precipitates at different ethanol concentrations to separate the two polysaccharides, and obtaining crude fucoidan and alginate. This method also requires the consumption of a large amount of precipitant, and the purity of the alginate product cannot be guaranteed. Summary of the invention

[0006] The present invention aims at the deficiencies in the prior art and provides a method for preparing an anion exchange resin film and its application in extracting polysaccharides, thereby solving the problem that the traditional extraction method can only extract one polysaccharide or multiple polysaccharides at the same time, which consumes a lot of organic solvents.

[0007] The technical solution of the present invention to solve the above technical problem is as follows: a method for preparing an anion exchange resin film, wherein the anion exchange resin film is prepared by the following preparation method:

[0008] 1,6-Diiodohexane and trimethylamine react in a solvent system to obtain a small molecule A, wherein the small molecule A is: ;

[0009] N,N,N',N'-tetramethyl-1,6-hexanediamine reacts with small molecule A in a solvent system to obtain a quaternary ammonium salt small molecule B, wherein the quaternary ammonium salt small molecule B is:

[0010] ;

[0011] After the brominated PPO and NaN3 are reacted in a solvent system, the quaternary ammonium salt small molecule B is added to react to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain. The product C is:

[0012] ;

[0013] Product C is dissolved in an organic solvent, and PPh3 is added, heated to react, then cooled, and isocyanate is added to the system to react. After the reaction is completed, product D is obtained. Product D is:

[0014] ;

[0015] The product D is separated, coated and dried to obtain an anion exchange resin film.

[0016] Furthermore, the degree of substitution of bromine in the brominated PPO is not less than 28%.

[0017] Furthermore, the reaction temperature of 1,6-diiodohexane and trimethylamine is 20-30°C; the reaction temperature of N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is 20-30°C; and the polymerization temperature of brominated PPO and NaN3 is 60-80°C.

[0018] Furthermore, the product C is dissolved in an organic solvent, and PPh3 is added, heated to 60-80°C for reaction, then cooled to 15-25°C, and isocyanate is added to the system for reaction.

[0019] Furthermore, the solvent used in the reaction of 1,6-diiodohexane and trimethylamine is THF;

[0020] The solvent used in the reaction between N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is DMF;

[0021] The solvent used in the bromination of PPO and NaN3 reaction is NMP;

[0022] The organic solvent used in the preparation of product D from product C is a mixed solvent of NMP, DMF and chloroform, wherein the volume ratio of NMP, DMF and chloroform in the mixed solvent is 25: (10-20): (5-10).

[0023] Furthermore, the mass ratio of brominated PPO and NaN3 is (10-15):1; the mass ratio of brominated PPO and quaternary ammonium salt small molecule B is (1.2-2.1):1;

[0024] The mass ratio of product C and PPh3 is (3.5-7):1; the mass ratio of product C and isocyanate is (11~21):1.

[0025] The present invention also discloses a process for extracting polysaccharides from seaweed, which comprises:

[0026] S1. Pre-treating, digesting and diluting the seaweed;

[0027] S2, taking the diluted supernatant, adding the anion exchange resin membrane of the present invention for adsorption, and then performing solid-liquid separation, and collecting the filtrate and the filter residue respectively;

[0028] S3, subjecting the filtrate to calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation and drying operations to obtain sodium alginate;

[0029] The filter residue is added to a NaOH solution for soaking, and the solid and liquid are separated to obtain a clear liquid; anhydrous ethanol is added to the clear liquid, and the precipitated solid is collected and dried to obtain fucoidan.

[0030] Furthermore, in step S2, the amount of the anion exchange resin membrane used is 0.01%-0.1% of the mass of the supernatant.

[0031] Furthermore, in step S3, the NaOH solution is a NaOH aqueous solution with a concentration of 0.8-1.2 mol / L, and the amount of the NaOH solution used is 1-3 times the mass of the filter residue.

[0032] Furthermore, in step S2, the anion exchange resin membrane is added to the supernatant and allowed to stand for adsorption for 18-24 hours;

[0033] In step S3, the filter residue is soaked in the NaOH solution for 2-6 hours.

[0034] The beneficial effects of the present invention are:

[0035] The present invention prepares an alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains to adsorb fucoidan anions in a diluted supernatant. The filtrate after the adsorption treatment contains almost no fucoidan, which can effectively reduce the fucoidan content in a sodium alginate product, improve the purity of the sodium alginate product, and increase its spinnability.

[0036] The anion exchange resin of the present invention is a polymer compound with a functional group (active group with exchange ions), a reticular structure, and insolubility. It is composed of elements such as carbon, hydrogen, oxygen, nitrogen, and sulfur. These elements are respectively connected to the functional groups and exchangeable ions in the polymer skeleton of the polymer compound, and ion exchange occurs during contact with the solution. Although the resin is insoluble in aqueous solution, it can form a movable ion layer, and the counterions in the solution can be ion exchanged with it in the movable ion layer. Fucoidan contains natural sulfate groups, and the sodium alginate molecular chain contains carboxyl groups. Therefore, the anion exchange resin film of the present invention preferentially adsorbs fucoidan. If the amount is properly controlled, the extraction rate of sodium alginate will hardly be affected. The reaction of the anion exchange resin film adsorbing anions is a reversible reaction. The adsorption capacity of the ion exchange resin for hydroxide ions is stronger than that of other anions, so the fucoidan anions can be replaced by hydroxide ions to achieve the purpose of recycling and reduce costs. The adsorption of fucoidan by the anion exchange resin membrane is equivalent to enrichment, and only a small amount of NaOH needs to be added during the replacement process, so only a small amount of ethanol is needed to achieve the complete precipitation of fucoidan.

[0037] The anion exchange resin film prepared by the invention contains urea side chains and a large number of hydrogen bonds between molecular chains, so it has good alkali stability and can be used for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the quaternary ammonium salt small molecule B described in Example 1;

[0039] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the product D described in Example 1. DETAILED DESCRIPTION

[0040] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.

[0042] A method for preparing an anion exchange resin film, wherein the anion exchange resin film is prepared by the following preparation method:

[0043] 1,6-Diiodohexane and trimethylamine react in a solvent system to obtain a small molecule A, wherein the small molecule A is: ;

[0044] N,N,N',N'-tetramethyl-1,6-hexanediamine reacts with small molecule A in a solvent system to obtain a quaternary ammonium salt small molecule B, wherein the quaternary ammonium salt small molecule B is:

[0045] ;

[0046] After the brominated PPO and NaN3 (sodium azide) are reacted in a solvent system (NaN3 replaces the bromine on the brominated PPO to generate an N3 group), the quaternary ammonium salt small molecule B is added for polymerization reaction to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain. The product C is:

[0047] ;

[0048] Product C is dissolved in an organic solvent, and PPh3 (triphenylphosphine) is added, and the reaction is heated (PPh3 reduces the N3 azide group in product C to an amino group, and reacts with the amino group after adding isocyanate to form a urea bond), then the temperature is lowered, and isocyanate is added to the system for reaction. After the reaction is completed, product D is obtained. Product D is:

[0049] ;

[0050] The product D is separated, coated and dried to obtain an anion exchange resin film.

[0051] Specifically, the degree of substitution of bromine in the brominated PPO is not less than 28%.

[0052] Preferably, the degree of substitution of bromine in the brominated PPO is 28% to 34%;

[0053] More preferably, the degree of substitution of bromine in the brominated PPO is 34%.

[0054] The brominated PPO is obtained by homemade, and the preparation method is as follows:

[0055] Dissolve PPO (polyphenylene ether) in CCl4 (carbon tetrachloride) solvent, add N-bromosuccinimide, heat to 60°C, add AIBN (azobisisobutyronitrile), react for 4 hours, and precipitate the product with ice methanol to obtain brominated PPO.

[0056] The specific reaction principle is as follows:

[0057] ;

[0058] Wherein, x and y are both integers, and the degree of substitution of bromine in the brominated PPO is: the ratio of the molar number of repeating units in which the hydrogen atoms on the methyl groups in the brominated PPO are replaced by Br to the molar number of all repeating units in PPO (the degree of substitution of the final brominated PPO product can be determined by NMR).

[0059] Among them, the mass ratio of PPO, N-bromosuccinimide and azobisisobutyronitrile is 1: (0.42~0.54): (0.19~0.23).

[0060] The PPO used in the preparation of brominated PPO in the present invention is: Asahi Chemical 500H from Japan.

[0061] According to the above method, brominated PPO with a bromine substitution degree of 34% and brominated PPO with a bromine substitution degree of 28% were prepared and used in the subsequent specific examples.

[0062] In the subsequent comparative example 3, the mass ratio of the raw materials PPO, N-bromosuccinimide and azobisisobutyronitrile for synthesizing brominated PPO with a bromine substitution degree of 20% is 1:0.3:0.14.

[0063] Specifically, the reaction temperature of 1,6-diiodohexane and trimethylamine is 20-30°C; the reaction temperature of N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is 20-30°C; and the polymerization temperature of brominated PPO and NaN3 is 60-80°C.

[0064] Specifically, the product C is dissolved in an organic solvent, and PPh3 is added, heated to 60-80°C for reaction, then cooled to 15-25°C, and isocyanate is added to the system for reaction.

[0065] Specifically, the solvent used in the reaction of 1,6-diiodohexane and trimethylamine is THF;

[0066] The solvent used in the reaction between N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is DMF;

[0067] The solvent used in the bromination of PPO and NaN3 reaction is NMP;

[0068] The organic solvent used in the preparation of product D from product C is a mixed solvent of NMP, DMF and chloroform, wherein the volume ratio of NMP, DMF and chloroform in the mixed solvent is 25: (10-20): (5-10).

[0069] Specifically, the molar ratio of 1,6-diiodohexane and trimethylamine can be designed according to the molar ratio of the reaction equation, and the molar ratio of 1,6-diiodohexane and trimethylamine is about 1:1;

[0070] The molar ratio of N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A can be designed according to the molar ratio of the reaction equation. The molar ratio of N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is about 1:1;

[0071] The mass ratio of brominated PPO and NaN3 is (10-15):1; the mass ratio of brominated PPO and quaternary ammonium salt small molecule B is (1.2-2.1):1;

[0072] The mass ratio of product C and PPh3 is (3.5-7):1; the mass ratio of product C and isocyanate is (11~21):1.

[0073] More specifically, the coating process adopts a conventional coating method. First, the glass plate is washed and soaked in an alkali tank for 8 hours, and then it is thoroughly washed with deionized water. The oven temperature is set to 80°C, the glass plate is placed in, and it is leveled at the same time, baked for 6 hours, taken out, and cooled naturally. The prepared polymer is dripped onto the glass plate with a plastic dropper, and a glass rod with copper wires at both ends is used for coating. Then the glass plate is placed in an oven, the temperature is set to 80°C, and it is baked for 12 hours. After 12 hours, it is placed in a vacuum oven, the temperature is set to 80°C, and the vacuum is applied for 3 hours. It is taken out and placed in a NaCl solution with a concentration of 2 mol / L, and soaked twice, each time for 24 hours, and finally soaked in clean water for 12 hours.

[0074] A process for extracting polysaccharides from seaweed, the process comprising:

[0075] S1. Pre-treating, digesting and diluting the seaweed;

[0076] S2, taking the diluted supernatant, adding the anion exchange resin membrane for adsorption, and then performing solid-liquid separation, and collecting the filtrate and the filter residue respectively;

[0077] S3, subjecting the filtrate to calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation and drying operations to obtain sodium alginate;

[0078] The filter residue is added to a NaOH solution for soaking, and the solid and liquid are separated to obtain a clear liquid; anhydrous ethanol is added to the clear liquid, and the precipitated solid is collected and dried to obtain fucoidan.

[0079] Specifically, in step S2, the amount of the anion exchange resin membrane used is 0.01%-0.1% of the mass of the supernatant.

[0080] Specifically, in step S3, the NaOH solution is a NaOH aqueous solution with a concentration of 0.8-1.2 mol / L, and the amount of the NaOH solution used is 1-3 times the mass of the filter residue; the amount of the anhydrous ethanol added is 1-3 times the mass of the filter residue.

[0081] Specifically, in step S2, the anion exchange resin membrane is added to the supernatant and allowed to stand for adsorption for 18-24 hours;

[0082] In step S3, the filter residue is soaked in the NaOH solution for 2-6 hours.

[0083] The pretreatment, digestion and dilution of the seaweed in step S1 and the calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation and drying of the filtrate in step S3 all adopt the method in Chinese patent CN117659223B. The specific operations in the embodiment of the present invention are as follows:

[0084] Pretreatment: Use a crusher to crush the dried kelp, filter it with a 5-mesh sieve, wash the sieved kelp particles with deionized water to remove impurities such as sand on the surface, and then soak them in deionized water for 6 hours.

[0085] Digestion: Add 3% sodium carbonate solution to the soaked kelp particles, the amount added is 10 times the mass of the kelp particles, control the system temperature at 60°C, and stir for 3 hours.

[0086] Dilution: Add deionized water 200 times the mass of dry kelp particles to the digested paste-like viscous material, stir to obtain a suspension, add 1% dilute hydrochloric acid to adjust the pH value to neutral, and let it stand for 6 hours.

[0087] Calcium coagulation: ozone bleaching is introduced into the filtrate, and air bubbles are installed at the ventilation pipe mouth to gather a large number of bubbles on the surface of the supernatant, and the air flow rate is controlled to be 11.2g / h per liter of supernatant. After bleaching for 15 minutes, ventilation is maintained, and a 15% calcium chloride solution is sprayed on the surface of the supernatant using a spray device. The flow rate of calcium chloride solution spraying per liter of supernatant is controlled at 0.2L / min, and a scraper is used to continuously scrape the calcium alginate flocculent solids into the collection device, and the calcium alginate flocculent solids are poured into a fluidized bed inclined at 15° to separate the calcium alginate. Subsequently, the calcium alginate flocculent solids are collected and placed in a freezer at -15°C for 6 hours, and the frozen calcium alginate is taken out, thawed and filtered at room temperature to obtain a porous structure calcium alginate.

[0088] Decalcification: The frozen and thawed calcium alginate is placed in a decalcification tank for three-stage continuous decalcification. The first decalcification tank uses the waste acid water of the second decalcification, the second decalcification tank uses the waste acid water of the third decalcification, and the third decalcification tank uses 1% dilute hydrochloric acid. After the three-stage decalcification, it enters the water washing tank. The decalcification time of each stage is 15 minutes.

[0089] Washing: Add enough deionized water to the washing tank, the amount of deionized water is 80 times the mass of alginate, stir for 15 minutes and then replace the deionized water, repeat the above steps 3 times, and dehydrate using a spiral dehydrator;

[0090] Neutralization, alcohol precipitation, and drying: Soak the dehydrated alginate in 95% ethanol, the mass of which is 15 times that of the alginate. Then, drop a NaOH solution (40% by mass sodium hydroxide solution) into the alginate solution and stir. During this period, the pH value is continuously tested. After adjusting the pH value to neutral, the alginate solution is filtered to obtain a flocculent solid. The solid is dried and ground to obtain a sodium alginate powder product.

[0091] Example 1

[0092] A method for simultaneously extracting sodium alginate and fucoidan from seaweed, the specific steps of which are:

[0093] (1) Synthesis of an alkali-resistant anion exchange resin membrane having quaternary ammonium cationic side chains and urea side chains:

[0094] 3 g of trimethylamine THF solution (the mass concentration of trimethylamine in THF solution is 49 wt %) was slowly added to 17.3 g of 1,6-diiodohexane, and the mixture was reacted at 25° C. for 24 h to obtain small molecule A.

[0095] 19.8g of small molecule A was dissolved in 50mL of DMF solvent, 8.6g of N,N,N',N'-tetramethyl-1,6-hexanediamine was dissolved in 50mL of DMF solvent, and the DMF solution of small molecule A was slowly added dropwise, and the reaction was carried out at 25°C for 12h to obtain quaternary ammonium salt small molecule B; the nuclear magnetic resonance hydrogen spectrum of quaternary ammonium salt small molecule B is shown as follows Figure 1 As shown (NMR conditions: DMSO-d6, 600 MHz).

[0096] 2 g of brominated PPO with a substitution degree of 34% was dissolved in 50 mL of NMP, 0.154 g of NaN3 was added, the temperature was raised to 60°C, and the reaction was continued for 22 h. 1.423 g of quaternary ammonium salt small molecule B was added to the reaction, and the reaction was continued at 60°C for 22 h. Stirring was stopped to obtain a polymer solution, and the polymer solution was poured into acetone and precipitated for 10 minutes. After filtration, the filter residue was placed in a vacuum drying oven and dried to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain.

[0097] Weigh 3.4g of product C and dissolve it in a mixed solvent of NMP, DMF and chloroform (the volumes of NMP, DMF and chloroform are 25mL, 15mL and 8mL respectively), add 0.62g of PPh3, heat to 60℃ (N2 protection), stop heating after 2h, wait for the solution to cool to 20℃, add 0.201g of isocyanate, and react at 20℃, wait for the solution to become turbid, solid (product D) gradually precipitates, filter, coat and dry to obtain an alkali-resistant anion exchange resin film with quaternary ammonium cation side chains and urea side chains. The hydrogen nuclear magnetic resonance spectrum of product D is shown in Figure 2 As shown (NMR conditions: DMSO-d6, 600 MHz).

[0098] (2) Pre-treatment, digestion and dilution of seaweed.

[0099] (3) Take the diluted supernatant and add 0.01% of the mass of the supernatant to an alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains, let it stand for 24 hours, filter and collect the filtrate for calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation, and drying to extract high-quality sodium alginate.

[0100] (4) Collect the filter residue after filtering in step (3), add 1.2 mol / L NaOH solution with the same mass as the filter residue, soak for 4 h, and filter to obtain a clear liquid.

[0101] (5) Add anhydrous ethanol of the same mass as the residue in step (4) to the clear liquid, collect the precipitated solid, and dry it to obtain fucoidan.

[0102] Example 2

[0103] A method for simultaneously extracting sodium alginate and fucoidan from seaweed, the specific steps of which are:

[0104] (1) Synthesis of an alkali-resistant anion exchange resin membrane having quaternary ammonium cationic side chains and urea side chains:

[0105] 1.5 g of trimethylamine in THF solution (the mass concentration of trimethylamine in THF solution is 49 wt %) was slowly added to 8.65 g of 1,6-diiodohexane, and the mixture was reacted at 20° C. for 30 h to obtain small molecule A.

[0106] 9.92 g of small molecule A was dissolved in 50 mL of DMF solvent, 4.3 g of N,N,N',N'-tetramethyl-1,6-hexanediamine was dissolved in 50 mL of DMF solvent, and the DMF solution of small molecule A was slowly added dropwise, and the reaction was carried out at 20° C. for 12 h to obtain quaternary ammonium salt small molecule B.

[0107] 2 g of brominated PPO with a substitution degree of 34% was dissolved in 50 mL of NMP, 0.134 g of NaN3 was added, the temperature was raised to 80°C, and the reaction was continued for 28 h. 1.593 g of quaternary ammonium salt small molecule B was added to the reaction, and the reaction was continued at 80°C for 28 h. Stirring was stopped to obtain a polymer solution, and the polymer solution was poured into acetone and precipitated for 30 minutes. After filtration, the filter residue was placed in a vacuum drying oven and dried to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain.

[0108] Weigh 3.6 g of product C and dissolve it in a mixed solvent of NMP, DMF and chloroform (the volumes of NMP, DMF and chloroform are 25 mL, 20 mL and 5 mL respectively), add 0.524 g of PPh3, raise the temperature to 80°C (N2 protection), stop heating after heating for 4 hours, wait for the solution to cool to 25°C, add 0.175 g of isocyanate, and react at 25°C. Wait for the solution to become turbid and solid (product D) to gradually precipitate, filter and dry the film to obtain an alkali-resistant anion exchange resin membrane with quaternary ammonium cationic side chains and urea side chains.

[0109] (2) Pre-treatment, digestion and dilution of seaweed.

[0110] (3) Take the diluted supernatant and add 0.1% of the mass of the supernatant to an alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains, let it stand for 24 hours, filter and collect the filtrate for calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation, and drying to extract high-quality sodium alginate.

[0111] (4) Collect the filter residue after filtering in step (3), add 1 mol / L NaOH solution twice the mass of the filter residue, soak for 6 h, and filter to obtain a clear liquid.

[0112] (5) Add anhydrous ethanol twice the mass of the filter residue in step (4) to the clear liquid, collect the precipitated solid, and dry it to obtain fucoidan.

[0113] Example 3

[0114] A method for simultaneously extracting sodium alginate and fucoidan from seaweed, the specific steps of which are:

[0115] (1) Synthesis of an alkali-resistant anion exchange resin membrane having quaternary ammonium cationic side chains and urea side chains:

[0116] 1.5 g of trimethylamine in THF solution (the mass concentration of trimethylamine in THF solution is 49 wt %) was slowly added to 8.65 g of 1,6-diiodohexane, and the mixture was reacted at 30° C. for 28 h to obtain small molecule A.

[0117] 9.92 g of small molecule A was dissolved in 50 mL of DMF solvent, 4.3 g of N,N,N',N'-tetramethyl-1,6-hexanediamine was dissolved in 50 mL of DMF solvent, and the DMF solution of small molecule A was slowly added dropwise, and the reaction was carried out at 30° C. for 12 h to obtain quaternary ammonium salt small molecule B.

[0118] 2 g of brominated PPO with a substitution degree of 34% was dissolved in 50 mL of NMP, 0.2 g of NaN3 was added and the temperature was raised to 70°C, and the reaction was carried out for 24 h. 1.024 g of quaternary ammonium salt small molecule B was added to the reaction, and the reaction was continued at 70°C for 24 h. Stirring was stopped to obtain a polymer solution, and the polymer solution was poured into acetone and precipitated for 20 minutes. After filtration, the filter residue was placed in a vacuum drying oven and dried to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain.

[0119] Weigh 3 g of product C and dissolve it in a mixed solvent of NMP, DMF and chloroform (the volumes of NMP, DMF and chloroform are 25 mL, 10 mL and 10 mL respectively), add 0.8 g of PPh3, raise the temperature to 70°C (N2 protection), stop heating after heating for 3 hours, wait for the solution to cool to 15°C, add 0.262 g of isocyanate, and react at 15°C. Wait for the solution to become turbid and solid (product D) to gradually precipitate. Filter and dry the film to obtain an alkali-resistant anion exchange resin membrane with quaternary ammonium cationic side chains and urea side chains.

[0120] (2) Pre-treatment, digestion and dilution of seaweed.

[0121] (3) Take the diluted supernatant and add 0.1% of the mass of the supernatant to an alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains, let it stand for 18 hours, filter and collect the filtrate for calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation, and drying to extract high-quality sodium alginate.

[0122] (4) Collect the filter residue after filtering in step (3), add 0.8 mol / L NaOH solution three times the mass of the filter residue, soak for 2 h, and filter to obtain a clear liquid.

[0123] (5) Add three times the mass of anhydrous ethanol as the residue in step (4) to the clear liquid, collect the precipitated solid, and dry it to obtain fucoidan.

[0124] Example 4

[0125] A method for simultaneously extracting sodium alginate and fucoidan from seaweed, the specific steps of which are:

[0126] (1) Synthesis of an alkali-resistant anion exchange resin membrane having quaternary ammonium cationic side chains and urea side chains:

[0127] 3 g of trimethylamine THF solution (the mass concentration of trimethylamine in THF solution is 49 wt %) was slowly added to 17.3 g of 1,6-diiodohexane, and the mixture was reacted at 25° C. for 24 h to obtain small molecule A.

[0128] 19.8 g of small molecule A was dissolved in 50 mL of DMF solvent, 8.6 g of N,N,N',N'-tetramethyl-1,6-hexanediamine was dissolved in 50 mL of DMF solvent, and the DMF solution of small molecule A was slowly added dropwise, and the reaction was carried out at 25° C. for 12 h to obtain quaternary ammonium salt small molecule B.

[0129] 2 g of brominated PPO with a substitution degree of 28% was dissolved in 50 mL of NMP, 0.154 g of NaN3 was added, the temperature was raised to 60°C, and the reaction was continued for 22 h. 0.967 g of quaternary ammonium salt small molecule B was added to the reaction, and the reaction was continued at 60°C for 22 h. Stirring was stopped to obtain a polymer solution, and the polymer solution was poured into acetone and precipitated for 10 minutes. After filtration, the filter residue was placed in a vacuum drying oven and dried to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain.

[0130] Weigh 2.88 g of product C and dissolve it in a mixed solvent of NMP, DMF and chloroform (the volumes of NMP, DMF and chloroform are 25 mL, 15 mL and 8 mL respectively), add 0.62 g of PPh3, raise the temperature to 60°C (N2 protection), stop heating after heating for 2 hours, wait for the solution to cool to 15°C, add 0.201 g of isocyanate, and react at 15°C. Wait for the solution to become turbid and solid (product D) to gradually precipitate, filter, coat and dry to obtain an alkali-resistant anion exchange resin membrane with quaternary ammonium cationic side chains and urea side chains.

[0131] (2) Pre-treatment, digestion and dilution of seaweed.

[0132] (3) Take the diluted supernatant and add 0.05% of the mass of the supernatant to an alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains, let it stand for 18 hours, filter and collect the filtrate for calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation, and drying to extract high-quality sodium alginate.

[0133] (4) Collect the filter residue after filtration in step (3), add 1 mol / L NaOH solution equal to the mass of the filter residue, soak for 4 h, and filter to obtain a clear liquid.

[0134] (5) Add anhydrous ethanol of the same mass as the residue in step (4) to the clear liquid, collect the precipitated solid, and dry it to obtain fucoidan.

[0135] Comparative Example 1

[0136] Sodium alginate and fucoidan were simultaneously extracted from seaweed using the same method as in Example 1, except that the proportion of anion exchange resin membrane added in step (3) was increased. In this comparative example 1, 2% by weight of the supernatant of an alkali-resistant anion exchange resin membrane having quaternary ammonium cationic side chains and urea side chains was added in step (3).

[0137] Comparative Example 2

[0138] Sodium alginate and fucoidan were simultaneously extracted from seaweed using the same method as in Example 1, except that no anion exchange resin membrane was added. The specific process was as follows:

[0139] (1) Pre-treatment, digestion and dilution of seaweed.

[0140] (2) Take the diluted supernatant and perform calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation, and drying operations to extract sodium alginate.

[0141] (3) Adding the same mass of anhydrous ethanol as in Example 1 to the wastewater after calcium coagulation in step (2), collecting the precipitated solid, and drying to obtain fucoidan.

[0142] Comparative Example 3

[0143] Sodium alginate and fucoidan were simultaneously extracted from seaweed using the same method as in Example 1, except that the anion exchange resin membrane having a substitution degree of 34% and having quaternary ammonium cation side chains and urea side chains was replaced with an anion exchange resin membrane having a substitution degree of 20% and having quaternary ammonium cation side chains and urea side chains, and other operations were the same as in Example 1.

[0144] The yields of sodium alginate and fucoidan proposed in the above examples and comparative examples were determined and calculated, wherein the calculation methods of the yields of sodium alginate and fucoidan were respectively: sodium alginate yield = sodium alginate dry weight / seaweed dry weight; fucoidan yield = fucoidan dry weight / seaweed dry weight.

[0145] The strength of the spinning product is directly related to the purity of the sodium alginate product. The sodium alginate product extracted in the embodiment and the comparative example is spun to make brown algae fiber, and the strength of the brown algae fiber is tested using a universal testing machine. The spinning process is as follows: the extracted sodium alginate is dissolved in water to prepare a spinning solution with a mass fraction of 4%, the spinning solution is squeezed into a first coagulation bath with a mass fraction of 10% CaCl2 through a spinneret hole, the spinneret stretching multiple is 0.98 times, and the spinning solution enters a 5% CaCl2 stretching bath through the traction action of a traction roller, and the stretching multiple is 1.6 times to obtain a drafted fiber, and the brown algae fiber can be obtained after two washing processes and drying.

[0146] The extraction yields of sodium alginate and fucoidan and the strength performance data of brown algae fiber are shown in Table 1.

[0147] Table 1 Extraction yield of sodium alginate and fucoidan and strength properties of brown algae fiber

[0148]

[0149] From the above data, it can be seen that the anion exchange resin membrane of the present invention is used to extract sodium alginate and fucoidan, and a high yield of sodium alginate and fucoidan can be obtained at the same time, and the extracted fucoidan has good strength performance when prepared into brown algae fiber, which means that the extracted fucoidan has a high purity and is suitable for use in brown algae fiber.

[0150] In addition, the anion exchange resin membrane of the present invention contains urea side chains and contains a large number of hydrogen bonds between the molecular chains, so it has good alkaline stability and can be used for a long time. The filter residue after the soaking treatment in step (4) of Example 2 is washed with clean water and used again as an anion exchange resin membrane in the process of extracting sodium alginate and fucoidan from seaweed. It was found in the experiment that the anion exchange resin membrane was recycled 10 times. Each time it was used, the fucoidan yield was more than 4.8%, the sodium alginate yield was more than 16%, and the breaking strength of the brown algae fiber was not less than 2.4 cN / dtex. It can be seen that the anion exchange resin membrane of the present invention can be recycled for a long time and is very suitable for application in industrial production.

[0151] From the comparison of the data of Comparative Example 1 and Example 1, it can be seen that in Comparative Example 1, due to the excessive addition of the alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains, the alginate ions present in the clear liquid were adsorbed, resulting in a low yield of sodium alginate. Therefore, the use of the anion exchange resin membrane of the present invention is more conducive to obtaining a high yield of sodium alginate and fucoidan at the same time.

[0152] From the comparison of the data of Comparative Example 2 and Example 1, it can be seen that in Comparative Example 2, since no alkali-resistant anion exchange resin membrane having quaternary ammonium cation side chains and urea side chains was added to enrich the fucoidan, the fucoidan was dissolved in a large amount of clear liquid, and a small amount of ethanol could not achieve the complete precipitation of the fucoidan, so the fucoidan yield was low. In addition, the fucoidan existed in the calcium alginate hydrogel obtained after calcification, resulting in the final sodium alginate mixed with fucoidan, with poor purity, so the fucoidan fiber had a low breaking strength.

[0153] From the comparison of the data of Comparative Example 3 and Example 1, it can be seen that due to the decrease in the degree of substitution, the functional side chains of the anion exchange resin membrane having quaternary ammonium cationic side chains and urea side chains are reduced, resulting in the inability to completely adsorb the fucoidan anions in the clear liquid, the fucoidan yield is low, and the purity of the extracted sodium alginate is poor, and the strength of the brown algae fiber obtained by spinning is low.

[0154] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0155] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for preparing an anion exchange resin film, characterized in that: The anion exchange resin film is prepared by the following preparation method: 1,6-Diiodohexane and trimethylamine react in a solvent system to obtain a small molecule A, wherein the small molecule A is: ; N,N,N',N'-tetramethyl-1,6-hexanediamine reacts with small molecule A in a solvent system to obtain a quaternary ammonium salt small molecule B, wherein the quaternary ammonium salt small molecule B is: ; After the brominated PPO and NaN3 are reacted in a solvent system, the quaternary ammonium salt small molecule B is added to react to obtain a product C containing a quaternary ammonium cation side chain and an azide group side chain. The product C is: ; The degree of substitution of bromine in the brominated PPO is not less than 28%; Product C is dissolved in an organic solvent, and triphenylphosphine PPh3 is added, heated to react, then cooled, and isocyanate is added to the system to react. After the reaction is completed, product D is obtained. Product D is: ; The product D is separated, coated and dried to obtain an anion exchange resin film.

2. The method for preparing an anion exchange resin membrane according to claim 1, characterized in that: The reaction temperature of 1,6-diiodohexane and trimethylamine is 20-30°C; the reaction temperature of N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is 20-30°C; the reaction temperature of brominated PPO and NaN3 is 60~80°C.

3. The method for preparing an anion exchange resin membrane according to claim 1, characterized in that: The product C is dissolved in an organic solvent, and triphenylphosphine PPh3 is added, heated to 60-80°C for reaction, then cooled to 15-25°C, and isocyanate is added into the system for reaction.

4. The method for preparing an anion exchange resin membrane according to claim 1, characterized in that: The solvent used in the reaction of 1,6-diiodohexane and trimethylamine is THF; The solvent used in the reaction between N,N,N',N'-tetramethyl-1,6-hexanediamine and small molecule A is DMF; The solvent used in the bromination of PPO and NaN3 reaction is NMP; The organic solvent used in the preparation of product D from product C is a mixed solvent of NMP, DMF and chloroform, wherein the volume ratio of NMP, DMF and chloroform in the mixed solvent is 25: (10-20): (5-10).

5. The method for preparing an anion exchange resin membrane according to claim 1, characterized in that: The mass ratio of brominated PPO and NaN3 is (10-15):1; the mass ratio of brominated PPO and quaternary ammonium salt small molecule B is (1.2-2.1):1; The mass ratio of product C to triphenylphosphine PPh3 is (3.5-7):1; the mass ratio of product C to isocyanate is (11-21):

1.

6. A process for extracting polysaccharides from seaweed, characterized in that: The process is as follows: S1. Pre-treating, digesting and diluting the seaweed; S2, taking the diluted supernatant, adding the anion exchange resin membrane prepared by the preparation method according to any one of claims 1 to 5 for adsorption, and then performing solid-liquid separation, and collecting the filtrate and the filter residue respectively; the amount of the anion exchange resin membrane is 0.01%-0.1% of the mass of the supernatant; S3, subjecting the filtrate to calcium coagulation, decalcification, water washing, neutralization, alcohol precipitation and drying operations to obtain sodium alginate; The filter residue is added to a NaOH solution for soaking, and the solid and liquid are separated to obtain a clear liquid; anhydrous ethanol is added to the clear liquid, and the precipitated solid is collected and dried to obtain fucoidan.

7. A process for extracting polysaccharides from seaweed according to claim 6, characterized in that: In step S3, the NaOH solution is a NaOH aqueous solution with a concentration of 0.8-1.2 mol / L, and the amount of the NaOH solution used is 1-3 times the mass of the filter residue.

8. A process for extracting polysaccharides from seaweed according to claim 6, characterized in that: In step S2, the anion exchange resin membrane is added to the supernatant and allowed to stand for adsorption for 18-24 hours; In step S3, the filter residue is soaked in the NaOH solution for 2-6 hours.