A method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer
Para-aramid fibers were prepared by particle size sieving and differential dissolution processes, which solved the problem of uneven polymer particle size distribution, improved fiber performance, and enabled the environmentally friendly recycling of waste materials, making them suitable for industrial applications.
Patent Information
- Application Number
- CN202411095372.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
In existing technologies, uneven polymer particle size distribution leads to uneven dissolution, affecting the strength of para-aramid fibers. Furthermore, the treatment of spinning waste is not environmentally friendly and violates the requirements of sustainable development.
PPTA polymers are separated into different ranges by particle size sieving, and different varieties of para-aramid fibers are prepared by using differentiated dissolution processes and spinning conditions. Spinning waste is then reused to form an efficient recycling method.
It improves the strength and elongation of para-aramid fibers, realizes the efficient and comprehensive utilization of polymers and waste, meets environmental protection requirements, and is suitable for industrial transformation.
Smart Images

Figure CN118639350B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing para-aramid fiber by comprehensively utilizing PPTA polymer, and belongs to the technical field of para-aramid fiber materials. Background Art
[0002] Para-aramid fiber is widely used in aerospace, automobile, bulletproof equipment and other fields due to its high strength, high modulus and good heat resistance. However, with the continuous development of technology, the performance requirements of materials are getting higher and higher, especially in the field of safety protection, the requirements for the breaking strength of fibers are very strict; in addition, in the context of sustainable development, improving the comprehensive utilization of polymers and spinning waste has always been a research hotspot.
[0003] Poly(p-phenylene terephthalamide) (PPTA) polymer is an important precursor of para-aramid fiber, and its quality has an important influence on fiber performance. However, due to the complex polymerization process, the polymer particle size distribution is uneven and wide, but polymers with different particle size distributions are used as raw materials to enter the spinning process together, and large-particle polymers are difficult to dissolve in concentrated sulfuric acid. Prolonging the dissolution time will cause polymer degradation and affect fiber strength. In addition, small-particle polymers are prone to agglomeration during the dissolution process due to their large specific surface area, forming hard lumps, which affect fiber strength due to poor dissolution effect.
[0004] In addition, a small amount of waste is inevitably generated during the spinning process, part of which is the waste stock slurry produced during the spinning process, and part of which is the waste fibers with defects in the finished fibers. The traditional method of dealing with these wastes is to neutralize them and then incinerate them, but this process produces toxic gases, which harms the environment, and this method goes against the background of sustainable development in today's society.
[0005] Therefore, how to solve the problem of uneven polymer dissolution to improve the strength of para-aramid and how to enhance the comprehensive utilization of polymers and spinning waste have become the focus of current technical research. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing para-aramid fibers by comprehensively utilizing PPTA polymers. Different dissolution processes and spinning conditions are adopted for polymers with different particle sizes, so that different varieties of para-aramid fibers can be prepared by differentially using polymers with different particle sizes.
[0007] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing para-aramid fiber by comprehensively utilizing PPTA polymer, the method comprising: screening the PPTA polymer raw material for particle size, screening out PPTA polymer with a particle size range of 420-840 μm to prepare high-strength para-aramid fiber; screening out PPTA polymer with a particle size range of <420 μm and >840 μm to prepare high-elongation para-aramid fiber;
[0008] The monofilament fineness of the high-strength para-aramid fiber is 1D-2D, and the multifilament fineness is 200D-2000D; the tensile strength of the high-strength para-aramid fiber is ≥22 cN·dtex -1 (Among them, the tensile strength of superior products is ≥23.5 cN·dtex -1 ), elongation at break 3.7±0.5%, modulus 85±20 GPa;
[0009] The monofilament fineness of the high-elongation para-aramid fiber is 1D-2.5D, and the multifilament fineness is 150D-3000D; the elongation at break of the high-elongation para-aramid fiber is ≥4.5%.
[0010] Furthermore, the IV value of the PPTA polymer raw material is 5.5-7.5 dL / g, the test medium for the IV value of the PPTA polymer raw material is concentrated sulfuric acid, the dissolution temperature is 80°C, and the test temperature is 30°C.
[0011] Furthermore, a PPTA polymer with a particle size range of 420-840 μm is mixed and dissolved with concentrated sulfuric acid to obtain a liquid crystal spinning solution with a mass concentration of 19.8-20.5%, a dissolution temperature of 85-87°C, and a dissolution time of 1-2 h; the liquid crystal spinning solution is filtered, degassed, and filtered twice, then extruded from a spinneret, and coagulated to obtain the high-strength para-aramid fiber.
[0012] Furthermore, the liquid crystal spinning solution is initially filtered through a 15-20 μm sintered felt filter, and after filtration, the liquid crystal spinning solution is vacuum degassed through a degassing tower, and then secondary filtered through a 3-8 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement to prepare high-strength para-aramid fiber.
[0013] Furthermore, the liquid crystal spinning solution is extruded from the spinneret and then enters a low-temperature coagulation bath for coagulation and forming. The temperature of the low-temperature coagulation bath is 2-6°C. A skin-core structure is formed in the low-temperature coagulation bath to enhance the fiber strength, and then high-strength para-aramid fiber is obtained through post-processing.
[0014] Further, PPTA polymers with a particle size range of <420 μm and >840 μm are mixed and dissolved in concentrated sulfuric acid at a dissolution temperature of 87-88°C for a dissolution time of 1.5-2.5 h to form a spinning solution with a concentration of 19.5-20.5%; wherein the mass ratio of the PPTA polymer with a particle size range of <420 μm to the PPTA polymer with a particle size range of >840 μm is (1-4):1;
[0015] The spinning solution is degassed and filtered, extruded from a spinneret, and solidified to obtain the high-elongation para-aramid fiber.
[0016] Furthermore, the spinning solution is vacuum degassed in a degassing tower, filtered through a 3-10 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement to prepare high-elongation para-aramid fiber.
[0017] Furthermore, the spinning solution is extruded from the spinneret and then enters a high-temperature coagulation bath for coagulation and molding, the temperature of the coagulation bath is 21-27° C., and then post-processed to obtain high-elongation para-aramid fibers.
[0018] Furthermore, the waste stock solution slurry and waste silk generated in the process of preparing the high-strength para-aramid fiber and the high-elongation para-aramid fiber are redissolved in concentrated sulfuric acid to form a low-concentration stock solution with a mass concentration of 5-10%, and then the PPTA polymer raw material before screening is added to the low-concentration stock solution to obtain a liquid crystal spinning stock solution with a mass concentration of 19.5-20.4%. After degassing and filtering, the liquid crystal spinning stock solution is extruded from a spinneret and coagulated to obtain ordinary para-aramid fiber; the ordinary para-aramid fiber has a monofilament fineness of 1D-2D and a multifilament fineness of 200D-2000D; the tensile strength of the ordinary para-aramid fiber is ≥18 cN·dtex -1 (The tensile strength of superior products is ≥20 cN·dtex -1 ), elongation at break 3.5±1.0%, modulus 85±20 GPa.
[0019] Furthermore, when the waste stock solution slurry block and waste silk are dissolved in concentrated sulfuric acid, the dissolution temperature is 90-95° C. and the dissolution time is 2-2.5 h;
[0020] The liquid crystal spinning stock solution is vacuum degassed in a degassing tower, filtered through a 5-8 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement; the liquid crystal spinning stock solution is extruded from a spinneret and then enters a coagulation bath for forming, the coagulation bath temperature is 5-8°C, and then post-processed to obtain ordinary para-aramid fiber.
[0021] The beneficial effects of the present invention are:
[0022] The method of the present invention improves the homogeneity of the stock solution by screening the polymer particle size, and polymers in different particle size ranges are used to differentially prepare different types of aramid fibers, thereby improving the strength of the aramid fibers. At the same time, the waste stock solution slurry and waste fibers generated during the spinning process are reused to achieve efficient recycling of polymers and waste. Through the present invention, the strength of para-aramid fibers can be improved, and the comprehensive and efficient recycling of polymers and waste can be achieved.
[0023] The preparation method of the invention is simple and stable, has low cost, good product performance, high comprehensive utilization rate of polymers, recyclable waste, and is suitable for industrial transformation and upgrading. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a process flow chart of the method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer. DETAILED DESCRIPTION
[0025] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0027] like Figure 1 As shown, a method for preparing para-aramid fiber by comprehensively utilizing PPTA polymer is provided, wherein the method comprises: screening the PPTA polymer raw material for particle size, screening out PPTA polymer with a particle size range of 420-840 μm to prepare high-strength para-aramid fiber; screening out PPTA polymer with a particle size range of <420 μm and >840 μm to prepare high-elongation para-aramid fiber;
[0028] The monofilament fineness of the high-strength para-aramid fiber is 1D-2D, and the multifilament fineness is 200D-2000D; the tensile strength of the high-strength para-aramid fiber is ≥22 cN·dtex -1 , the tensile strength of superior products is ≥23.5 cN·dtex -1 , elongation at break 3.7±0.5%, modulus 85±20 GPa;
[0029] The monofilament fineness of the high-elongation para-aramid fiber is 1D-2.5D, and the multifilament fineness is 150D-3000D; the elongation at break of the high-elongation para-aramid fiber is ≥4.5%.
[0030] Specifically, the IV value of the PPTA polymer raw material is 5.5-7.5 dL / g, and the test medium for the IV value of the PPTA polymer raw material is concentrated sulfuric acid, the dissolution temperature is 80° C., and the test temperature is 30° C. The mass concentration of the concentrated sulfuric acid is not less than 98%.
[0031] More specifically, under the action of centrifugal force in the airflow classifier, the PPTA polymer raw material with a particle size of less than 420 μm enters the bag dust collector for collection, and the material with a particle size of more than 420 μm enters the lower end discharge port; further, an 840 μm screen is set at the lower end discharge port, so that the material with a particle size between 420-840 μm can pass through the screen and be blown to the silo by the fan for standby; the material with a particle size of more than 840 μm cannot pass through the screen and is collected separately at the lower end discharge port. The PPTA polymer is classified by the airflow classification system, and the polymer of the target particle size can be obtained by adjusting the frequency and speed of the classification wheel, thereby realizing the screening and collection of polymers of different particle sizes.
[0032] Specifically, a PPTA polymer with a particle size range of 420-840 μm is mixed and dissolved with concentrated sulfuric acid (mass concentration ≥ 98%) to obtain a liquid crystal spinning solution with a mass concentration of 19.8-20.5%, a dissolution temperature of 85-87°C, and a dissolution time of 1-2 hours; the liquid crystal spinning solution is filtered, degassed, and filtered twice, and then extruded from a spinneret by a metering pump, and coagulated to obtain the high-strength para-aramid fiber. Among them, the secondary filtration operation can make the spinning solution more uniform, improve the fiber strength, and also extend the service life of the filter element.
[0033] Specifically, the liquid crystal spinning solution is initially filtered through a 15-20 μm sintered felt filter, and after filtration, the liquid crystal spinning solution is vacuum degassed through a degassing tower with a vacuum degree controlled at 1-3 mmHg, and then filtered for a second time through a 3-8 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement to prepare high-strength para-aramid fiber.
[0034] Specifically, the liquid crystal spinning solution is extruded from a spinneret and then enters a low-temperature coagulation bath for coagulation and forming. The temperature of the low-temperature coagulation bath is 2-6°C. A skin-core structure is formed in the low-temperature coagulation bath to enhance the fiber strength, and then high-strength para-aramid fiber is obtained through post-processing.
[0035] More specifically, in an embodiment of the present invention, the low-temperature coagulation bath is a dilute sulfuric acid aqueous solution (containing 2-5% sulfuric acid by mass); when preparing high-strength para-aramid fiber, the post-treatment includes neutralization, washing, drying, heat setting, oiling, winding and other steps, wherein the drying temperature is 100-150°C, and the heat setting temperature is 150-280°C.
[0036] Specifically, PPTA polymers with a particle size range of <420 μm and >840 μm are mixed and dissolved in concentrated sulfuric acid at a dissolution temperature of 87-88°C for a dissolution time of 1.5-2.5 h to form a spinning solution with a concentration of 19.5-20.5%; wherein the mass ratio of the PPTA polymer with a particle size range of <420 μm to the PPTA polymer with a particle size range of >840 μm is (1-4):1;
[0037] The spinning solution is degassed and filtered, extruded from a spinneret by a metering pump, and coagulated to obtain the high-elongation para-aramid fiber.
[0038] Specifically, the spinning solution is vacuum degassed in a degassing tower with the vacuum degree controlled at 1-3 mmHg, and then filtered through a 3-10 μm sintered felt before being transported to each spinning position through a split pipeline arrangement to prepare high-elongation para-aramid fiber.
[0039] Specifically, the spinning solution is extruded from a spinneret and then enters a high-temperature coagulation bath for coagulation and molding, the temperature of the coagulation bath is 21-27° C., and then post-processed to obtain high-elongation para-aramid fibers.
[0040] More specifically, in an embodiment of the present invention, the high-temperature coagulation bath is a dilute sulfuric acid aqueous solution (containing 1-10% sulfuric acid by mass); when preparing high-elongation para-aramid fiber, the post-treatment includes neutralization, washing, drying, heat setting, oiling, winding and other steps, wherein the drying temperature is 100-200°C, and the heat setting temperature is 150-300°C.
[0041] Specifically, the waste stock solution slurry and waste silk generated in the process of preparing the high-strength para-aramid fiber and the high-elongation para-aramid fiber are redissolved in concentrated sulfuric acid to form a low-concentration stock solution with a mass concentration of 5-10%, and then the PPTA polymer raw material before screening is added to the low-concentration stock solution to obtain a liquid crystal spinning stock solution with a mass concentration of 19.5-20.4%. After the liquid crystal spinning stock solution is degassed and filtered, it is extruded from a spinneret and coagulated to obtain a common para-aramid fiber; the common para-aramid fiber has a monofilament fineness of 1D-2D and a multifilament fineness of 200D-2000D; the tensile strength of the common para-aramid fiber is ≥18 cN·dtex -1 , the tensile strength of superior products is ≥20 cN·dtex -1 , the elongation at break is 3.5±1.0%, and the modulus is 85±20 GPa.
[0042] Specifically, when the waste stock solution slurry block and waste silk are dissolved in concentrated sulfuric acid, the dissolution temperature is 90-95° C. and the dissolution time is 2-2.5 h;
[0043] The liquid crystal spinning stock solution is vacuum degassed in a degassing tower, the vacuum degree of which is controlled at 1-3 mmHg, and then filtered through a 5-8 μm sintered felt and transported to each spinning position through a split pipeline arrangement; the liquid crystal spinning stock solution is extruded from a spinneret by a metering pump and then enters a coagulation bath for forming, the coagulation bath temperature is 5-8°C, and then post-processed to obtain ordinary para-aramid fiber.
[0044] More specifically, in an embodiment of the present invention, the coagulation bath is a dilute sulfuric acid aqueous solution (containing 5-10% sulfuric acid by mass); when preparing ordinary para-aramid fiber, the post-treatment includes neutralization, washing, drying, heat setting, oiling, winding and other steps, wherein the drying temperature is 150-200°C, and the heat setting temperature is 250-420°C.
[0045] Example 1
[0046] A method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer, specifically comprising:
[0047] S1. The poly(p-phenylene terephthalamide) (PPTA) polymer with an IV value of 5.5-7.5 dL / g was screened by the airflow classification system. Under the action of centrifugal force in the airflow classifier, the material with a particle size of <420 μm entered the bag dust collector for collection. The measured polymer IV value was 6.8-7.5 dL / g, with a coefficient of variation of 0.9%; the material with a particle size of >420 μm entered the lower end discharge port, and a 840 μm screen was further set at the lower end discharge port so that the material with a particle size between 420-840 μm could pass through the screen and was blown to the silo by a fan for standby use. The measured polymer IV value was 6.2-6.8 dL / g, with a coefficient of variation of 1.1%; the material with a particle size of >840 μm could not pass through the screen and was collected separately at the lower end discharge port. The measured polymer IV value was 5.5-6.2 dL / g, with a coefficient of variation of 1.0%.
[0048] S2. The polymer with a particle size range of 420-840 μm and concentrated sulfuric acid with a concentration of 98% are fully dissolved at a dissolution temperature of 85°C and a dissolution time of 1.5 h. After dissolution, a uniform liquid crystal spinning solution with a concentration of 20% is formed. The liquid crystal spinning solution is initially filtered through a 15 μm sintered felt filter. After filtration, the solution is vacuum degassed through a degassing tower with a vacuum degree controlled at 2 mmHg. After secondary filtration through a 5 μm sintered felt, the solution is transported to each spinning position through a split pipeline arrangement. After the solution is extruded from the spinneret, it enters a low-temperature coagulation bath at 5°C for rapid coagulation and molding, forming a skin-core structure to enhance the fiber strength. After post-treatment, high-strength para-aramid fiber is obtained (wherein the low-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 3%, the drying temperature in the post-treatment process is 120°C, and the heat setting temperature is 200°C). The single-filament fineness is 1.5D and the multifilament fineness is 1000. D, fiber tensile strength 24.32 cN / dtex, elongation at break 3.76%, modulus 85 GPa.
[0049] S3. Polymers with particle sizes of <420 μm and >840 μm are mixed (wherein, the mass ratio of polymers with particle sizes of <420 μm and >840 μm is 3:1), and the doped polymers are dissolved in 98% concentrated sulfuric acid at a dissolution temperature of 87°C for 2 h to form a liquid crystal spinning solution with a concentration of 20%. The spinning solution is vacuum degassed in a degassing tower with a vacuum degree controlled at 2 mmHg, and then filtered through a 5 μm sintered felt and transported to each spinning position through a split pipeline arrangement. The solution is extruded from the spinneret and then enters a high-temperature coagulation bath at 27°C for coagulation and forming, and then post-treated to obtain high-elongation para-aramid fiber (wherein, the high-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 5%, the drying temperature in the post-treatment process is 150°C, and the heat setting temperature is 200°C), the single-filament fineness is 1 D, the multifilament fineness is 200 D, and the fiber strength is 19.14 cN / dtex, elongation at break 4.68%, modulus 84 GPa;
[0050] S4, the waste stock solution slurry and waste silk generated in steps S2, S3 and this step are redissolved in 98% concentrated sulfuric acid at a dissolution temperature of 90°C for 2.5 h to form a 5% low-concentration stock solution, and then a certain mass of unscreened PPTA polymer is added, and the mixture is mixed to form a liquid crystal spinning stock solution with a concentration of 20.1%. The spinning stock solution is vacuum degassed in a degassing tower with a vacuum degree controlled at 2 mmHg, and then filtered through an 8 μm sintered felt and transported to each spinning position through a split pipeline arrangement. The stock solution is extruded from the spinneret and enters a coagulation bath at 8°C for coagulation bath molding, and then post-treated to obtain ordinary para-aramid fiber (wherein the coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 7%, the drying temperature in the post-treatment process is 180°C, and the heat setting temperature is 300°C), the single fiber fineness is 1.5 D, and the multifilament fineness is 840 D, fiber strength 20.55 cN / dtex, elongation at break 3.52%, fiber modulus 87 GPa.
[0051] Example 2
[0052] A method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer, specifically comprising:
[0053] S1. The poly(p-phenylene terephthalamide) (PPTA) polymer with an IV value of 5.8-7.2 dL / g was screened by the airflow classification system. Under the centrifugal force in the airflow classifier, the material with a particle size of <420 μm entered the bag filter for collection. The measured polymer IV value was 6.7-7.2 dL / g, with a coefficient of variation of 1.2%; the material with a particle size of >420 μm entered the lower end discharge port, and a 840 μm screen was further set at the lower end discharge port so that the material with a particle size between 420-840 μm could pass through the screen and was blown to the silo by a fan for standby use. The measured polymer IV value was 6.1-6.7 dL / g, with a coefficient of variation of 0.7%; the material with a particle size of >840 μm could not pass through the screen and was collected separately at the lower end discharge port. The measured polymer IV value was 5.8-6.1 dL / g, with a coefficient of variation of 0.9%.
[0054] S2. The polymer with a particle size range of 420-840 μm and concentrated sulfuric acid with a concentration of 98% are fully dissolved at a dissolution temperature of 85°C and a dissolution time of 2 h. After dissolution, a uniform liquid crystal spinning solution with a concentration of 19.8% is formed. The liquid crystal spinning solution is initially filtered through a 15 μm sintered felt filter. After filtration, the solution is vacuum degassed through a degassing tower with a vacuum degree controlled at 1.8 mmHg. After secondary filtration through an 8 μm sintered felt, the solution is transported to each spinning position through a split pipeline arrangement. After the solution is extruded from the spinneret, it enters a low-temperature coagulation bath at 5°C for rapid coagulation and molding, forming a skin-core structure to enhance the fiber strength. After post-treatment, high-strength para-aramid fiber is obtained (wherein the low-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 2%, the drying temperature in the post-treatment process is 100°C, and the heat setting temperature is 150°C). The single-filament fineness is 2 D, the multifilament fineness is 2000 D, and the fiber tensile strength is 24.85 cN / dtex, elongation at break 3.72%, modulus 88 GPa.
[0055] S3. Polymers with particle sizes of <420 μm and >840 μm are mixed (wherein, the mass ratio of polymers with particle sizes of <420 μm and >840 μm is 2:1), and the doped polymers are dissolved in 98% concentrated sulfuric acid at a dissolution temperature of 87°C for 1.5 h to form a liquid crystal spinning solution with a concentration of 19.5%. The spinning solution is vacuum degassed in a degassing tower with a vacuum degree controlled at 1.8 mmHg, and then filtered through a 3 μm sintered felt and transported to each spinning position through a split pipeline arrangement. The solution is extruded from the spinneret and then enters a high-temperature coagulation bath at 25°C for coagulation and forming, and then post-treated to obtain high-elongation para-aramid fiber (wherein, the high-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 1%, the drying temperature in the post-treatment process is 100°C, and the heat setting temperature is 150°C), the single-filament fineness is 2 D, the multifilament fineness is 2000 D, and the fiber strength is 19.43 cN / dtex, elongation at break 4.75%, modulus 86 GPa;
[0056] S4, the waste stock solution slurry and waste silk generated in steps S2, S3 and this step are redissolved in 98% concentrated sulfuric acid at a dissolution temperature of 92°C and a dissolution time of 2.0 h to form a 7% low-concentration stock solution, and then a certain mass of unscreened PPTA polymer is added, and the mixture is mixed to form a liquid crystal spinning stock solution with a concentration of 20.4%. The spinning stock solution is vacuum degassed in a degassing tower, and the vacuum degree is controlled at 2 mmHg. After being filtered through an 8 μm sintered felt, it is transported to each spinning position through a split pipeline arrangement. After the stock solution is extruded from the spinneret, it enters a 6°C coagulation bath for coagulation bath molding, and then post-processed to obtain a common para-aramid fiber (wherein the coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 5%, the drying temperature in the post-processing process is 150°C, and the heat setting temperature is 250°C), the single fiber fineness is 1.5 D, and the multifilament fineness is 840 D, fiber strength 20.78 cN / dtex, elongation at break 3.49%, fiber modulus 85 GPa.
[0057] Example 3
[0058] A method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer, specifically comprising:
[0059] S1. The poly(p-phenylene terephthalamide) (PPTA) polymer with an IV value of 6.0-7.4 dL / g was screened by the airflow classification system. Under the action of centrifugal force in the airflow classifier, the material with a particle size of <420 μm entered the bag filter for collection. The measured polymer IV value was 6.9-7.4 dL / g, with a coefficient of variation of 1.1%; the material with a particle size of >420 μm entered the lower end discharge port, and a 840 μm screen was further set at the lower end discharge port so that the material with a particle size between 420-840 μm could pass through the screen and was blown to the silo by a fan for standby use. The measured polymer IV value was 6.4-6.9 dL / g, with a coefficient of variation of 0.8%; the material with a particle size of >840 μm could not pass through the screen and was collected separately at the lower end discharge port. The measured polymer IV value was 6.0-6.4 dL / g, with a coefficient of variation of 1.2%.
[0060] S2. The polymer with a particle size range of 420-840 μm and concentrated sulfuric acid with a concentration of 98% are fully dissolved at a dissolution temperature of 87°C and a dissolution time of 2 h. After dissolution, a uniform liquid crystal spinning solution with a concentration of 20% is formed. The liquid crystal spinning solution is initially filtered through an 18 μm sintered felt filter. After filtration, the solution is vacuum degassed through a degassing tower with a vacuum degree controlled at 2.0 mmHg. After secondary filtration through a 5 μm sintered felt, the solution is transported to each spinning position through a split pipeline arrangement. After the solution is extruded from the spinneret, it enters a low-temperature coagulation bath at 4°C for rapid coagulation and molding, forming a skin-core structure to enhance the fiber strength. After post-treatment, high-strength para-aramid fiber is obtained (wherein the low-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 5%, the drying temperature during the post-treatment process is 150°C, and the heat setting temperature is 280°C). The single-filament fineness is 1.5 D and the multifilament fineness is 840 D, fiber tensile strength 24.97 cN / dtex, elongation at break 3.75%, modulus 84 GPa.
[0061] S3. Polymers with particle sizes of <420 μm and >840 μm are mixed (wherein, the mass ratio of polymers with particle sizes of <420 μm and >840 μm is 3:1), and the doped polymers are dissolved in 98% concentrated sulfuric acid at a dissolution temperature of 88°C for 2.0 h to form a liquid crystal spinning solution with a concentration of 20.5%. The spinning solution is vacuum degassed in a degassing tower with a vacuum degree controlled at 2.2 mmHg, and then filtered through an 8 μm sintered felt and transported to each spinning position through a split pipeline arrangement. The solution is extruded from the spinneret and then enters a high-temperature coagulation bath at 23°C for coagulation and forming, and then post-treated to obtain high-elongation para-aramid fiber (wherein, the high-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 10%, the drying temperature in the post-treatment process is 200°C, and the heat setting temperature is 300°C), the single yarn fineness is 1.5D, the multifilament fineness is 1000 D, and the fiber strength is 19.57 cN / dtex, elongation at break 4.73%, modulus 83GPa;
[0062] S4, the waste stock solution slurry blocks and waste silk generated in steps S2, S3 and this step are redissolved in 98% concentrated sulfuric acid at a dissolution temperature of 92°C and a dissolution time of 2.0 h to form a 5% low-concentration stock solution, and then a certain mass of unscreened PPTA polymer is added, and the mixture is mixed to form a liquid crystal spinning stock solution with a concentration of 19.8%. The spinning stock solution is vacuum degassed in a degassing tower, and the vacuum degree is controlled at 1.9 mmHg. After being filtered through a 5 μm sintered felt, it is transported to each spinning position through a split pipeline arrangement. After the stock solution is extruded from the spinneret, it enters a coagulation bath at 6°C for coagulation bath molding, and then post-processed to obtain a common para-aramid fiber (wherein the coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 10%, the drying temperature in the post-processing process is 200°C, and the heat setting temperature is 420°C), the single fiber fineness is 1 D, the multifilament fineness is 200 D, and the fiber strength is 20.64 cN / dtex, elongation at break 3.56%, fiber modulus 85 GPa.
[0063] Example 4
[0064] A method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer, specifically comprising:
[0065] S1. The poly(p-phenylene terephthalamide) (PPTA) polymer with an IV value of 6.2-7.5 dL / g was screened by the airflow classification system. Under the action of centrifugal force in the airflow classifier, the material with a particle size of <420 μm entered the bag dust collector for collection. The measured polymer IV value was 6.9-7.5 dL / g, with a coefficient of variation of 0.7%; the material with a particle size of >420 μm entered the lower end discharge port, and a 840 μm screen was further set at the lower end discharge port so that the material with a particle size between 420-840 μm could pass through the screen and was blown to the silo by a fan for standby use. The measured polymer IV value was 6.5-6.9 dL / g, with a coefficient of variation of 0.8%; the material with a particle size of >840 μm could not pass through the screen and was collected separately at the lower end discharge port. The measured polymer IV value was 6.2-6.5 dL / g, with a coefficient of variation of 0.8%.
[0066] S2. The polymer with a particle size range of 420-840 μm and concentrated sulfuric acid with a concentration of 98% are fully dissolved at a dissolution temperature of 87°C and a dissolution time of 2 h. After dissolution, a uniform liquid crystal spinning solution with a concentration of 20.5% is formed. The liquid crystal spinning solution is initially filtered through a 20 μm sintered felt filter. After filtration, the solution is vacuum degassed in a degassing tower with a vacuum degree controlled at 2.4 mmHg. After secondary filtration through a 3 μm sintered felt, the solution is transported to each spinning position through a split pipeline arrangement. After the solution is extruded from the spinneret, it enters a low-temperature coagulation bath at 6°C for rapid coagulation and molding, forming a skin-core structure to enhance the fiber strength. After post-treatment, high-strength para-aramid fiber is obtained (wherein the low-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 4%, the drying temperature in the post-treatment process is 120°C, and the heat setting temperature is 220°C). The single-filament fineness is 1.5 D and the multifilament fineness is 1000. D, fiber tensile strength 25.02 cN / dtex, elongation at break 3.74%, modulus 86 GPa.
[0067] S3. Polymers with particle sizes of <420 μm and >840 μm are mixed (wherein, the mass ratio of polymers with particle sizes of <420 μm and >840 μm is 4:1), and the doped polymers are dissolved in 98% concentrated sulfuric acid at a dissolution temperature of 88°C for 1.5 h to form a liquid crystal spinning solution with a concentration of 19.8%. The spinning solution is vacuum degassed in a degassing tower with a vacuum degree controlled at 2.0 mmHg, and then filtered through a 10 μm sintered felt and transported to each spinning position through a split pipeline arrangement. The solution is extruded from the spinneret and then enters a high-temperature coagulation bath at 21°C for coagulation and forming, and then post-treated to obtain high-elongation para-aramid fiber (wherein, the high-temperature coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 6%, the drying temperature in the post-treatment process is 150°C, and the heat setting temperature is 220°C), the single-filament fineness is 1.5D, the multifilament fineness is 840 D, and the fiber strength is 19.88 cN / dtex, elongation at break 4.80%, modulus 84GPa;
[0068] S4, the waste stock solution slurry and waste silk generated in steps S2, S3 and this step are redissolved in 98% concentrated sulfuric acid at a dissolution temperature of 90°C for 2.5 h to form a 10% low-concentration stock solution, and then a certain mass of unscreened PPTA polymer is added, and the mixture is mixed to form a liquid crystal spinning stock solution with a concentration of 19.5%. The spinning stock solution is vacuum degassed in a degassing tower, and the vacuum degree is controlled at 1.9 mmHg. After being filtered through a 5 μm sintered felt, it is transported to each spinning position through a split pipeline arrangement. After the stock solution is extruded from the spinneret, it enters a 5°C coagulation bath for coagulation bath molding, and then is post-treated to obtain a common para-aramid fiber (wherein the coagulation bath is a dilute sulfuric acid aqueous solution with a mass concentration of 6%, the drying temperature in the post-treatment process is 180°C, and the heat setting temperature is 320°C), the single fiber fineness is 1.5 D, and the multifilament fineness is 1000 D, fiber strength 20.77 cN / dtex, elongation at break 3.49%, fiber modulus 88 GPa.
[0069] Comparative Example 1
[0070] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not have the polymer particle size classification step in Example 1, that is, the unscreened polymer is used to prepare different types of para-aramid fibers, and other process conditions are the same as those in Example 1.
[0071] Comparative Example 2
[0072] The difference between Comparative Example 2 and Example 1 is that the dissolution temperature of polymers with different particle size distributions in concentrated sulfuric acid in steps S2, S3, and S4 of Comparative Example 2 is 90°C and the dissolution time is 2.5h, that is, the dissolution process of polymers with different particle size distributions is the same, and other process conditions are the same as those in Example 1.
[0073] Comparative Example 3
[0074] The difference between Comparative Example 3 and Example 1 is that the stock solutions of steps S2, S3 and S4 in Comparative Example 3 are all put into a 5° C. coagulation bath for coagulation and molding after being extruded through a spinneret, and the other process conditions are the same as those in Example 1.
[0075] Comparative Example 4
[0076] The difference between Comparative Example 4 and Example 1 is that the stock solutions of steps S2, S3 and S4 in Comparative Example 3 are all put into a 27° C. coagulation bath for coagulation and molding after being extruded through a spinneret, and the other process conditions are the same as those in Example 1.
[0077] Comparative Example 5
[0078] The difference between Comparative Example 5 and Example 1 is that the spinning solution in step S4 of Comparative Example 4 is entirely composed of waste solution slurry blocks and waste silk dissolved in concentrated sulfuric acid, without being doped with polymer, and other process conditions are the same as those in Example 1.
[0079] The process conditions involved in the above embodiments and comparative examples are shown in Tables 1 and 2 below.
[0080] Table 1 Process conditions of Examples 1-4
[0081]
[0082] Table 2 Process conditions of Comparative Examples 1-5
[0083]
[0084] The performance of the para-aramid fibers prepared in the above embodiments and comparative examples was tested. The specific test results are shown in Table 3 below, where the test methods involved refer to GB / T14344.
[0085] Table 3 Para-aramid fiber performance test data
[0086]
[0087] It can be seen from the experimental data of Examples 1 to 4 that the performance of different types of para-aramid fibers obtained in Examples 1 to 4 is good, the tensile strength of high-strength para-aramid fibers is greater than 23.5 cN / dtex, the elongation at break of high-elongation para-aramid fibers is greater than 4.5%, and the modulus of ordinary para-aramid fibers is greater than 85 GPa, in Examples 1 to 4, in step S1, the polymer is screened according to the particle size through an air flow classification system, and polymers in different particle size ranges are used to differentially prepare different types of aramid fibers, which can improve fiber performance; in steps S2, S3, and S4, polymers in different particle size ranges are subjected to different dissolution processes to obtain a uniform spinning solution, which solves the problem of insufficient dissolution and easy degradation of the polymer in concentrated sulfuric acid. In addition, after the solution is extruded through a spinneret, it enters a coagulation bath at different temperatures for finalization, and different types of aramid fibers are differentially prepared by polymers with different particle sizes, different dissolution processes, and different coagulation bath temperatures, which is conducive to the formation of high-performance fibers; in step S4, the waste solution slurry and waste silk generated during the spinning process of steps S2, S3, and S4 are reused, and they are re-dissolved in concentrated sulfuric acid with the polymer to form a spinning solution to prepare aramid fibers, which can achieve efficient and comprehensive recycling of polymers and waste.
[0088] It can be seen from Comparative Example 1 and Example 1 that Comparative Example 1 does not have the polymer particle size classification step in Example 1, that is, the unscreened polymer is used to prepare different types of para-aramid fibers, and the resulting high-strength para-aramid fibers and high-elongation para-aramid fibers have significantly decreased breaking properties. This is because the polymer particle size distribution is uneven and the particle size distribution is relatively wide, which results in uneven dissolution of the polymer in concentrated sulfuric acid, and the formed spinning solution has low uniformity, thereby affecting the performance of the fiber product.
[0089] It can be seen from Comparative Example 2 and Example 1 that, for polymers with different particle sizes, Comparative Example 2 does not adopt different dissolution processes, resulting in decreased fiber performance and difficulty in obtaining differentiated fibers of different varieties.
[0090] It can be seen from Comparative Examples 3-4 and Example 1 that, for different types of fibers, different coagulation bath temperatures were not used in Comparative Examples 3-4, resulting in decreased fiber performance and difficulty in obtaining differentiated fibers of different types.
[0091] It can be seen from Comparative Example 5 and Example 1 that the spinning solution in step S4 of Comparative Example 5 is entirely composed of waste solution slurry blocks and waste silk dissolved in concentrated sulfuric acid, without being doped with polymer, resulting in a sharp decline in the mechanical properties of the produced ordinary para-aramid fiber, with a tensile strength of only 18.14 cN / dtex. The reason is that the spinning solution is entirely composed of waste, and the waste contains irreversible microscopic defects, which causes the mechanical properties of the fiber product to decline.
[0092] The present invention improves the homogeneity of the stock solution by screening the polymer by particle size, and polymers in different particle size ranges are used to differentially prepare different types of aramid fibers, thereby improving the strength of the aramid fibers. At the same time, the waste stock solution slurry blocks and waste fibers generated during the spinning process are reused to achieve efficient recycling of polymers and waste. The method of the present invention can not only improve the strength of para-aramid fibers, but also achieve comprehensive and efficient recycling of polymers and waste. Moreover, the preparation method of the present invention is simple and stable, low in cost, good in product performance, high in comprehensive utilization rate of polymers, and waste can be recycled, and is suitable for industrial transformation and upgrading.
[0093] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0094] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer, characterized in that: The method comprises: screening the PPTA polymer raw material for particle size, screening out the PPTA polymer with a particle size range of 420-840 μm to prepare the high-strength para-aramid fiber; screening out the PPTA polymer with a particle size range of less than 420 μm and greater than 840 μm to prepare the high-elongation para-aramid fiber; The monofilament fineness of the high-strength para-aramid fiber is 1D-2D, and the multifilament fineness is 200D-2000D; the tensile strength of the high-strength para-aramid fiber is ≥22 cN·dtex -1 , elongation at break is 3.7±0.5%, modulus is 85±20GPa; The monofilament fineness of the high-elongation para-aramid fiber is 1D-2.5D, and the multifilament fineness is 150D-3000D; the elongation at break of the high-elongation para-aramid fiber is ≥4.5%; A PPTA polymer with a particle size range of 420-840 μm is mixed and dissolved with concentrated sulfuric acid to obtain a liquid crystal spinning solution with a mass concentration of 19.8-20.5%, a dissolution temperature of 85-87°C, and a dissolution time of 1-2 h; the liquid crystal spinning solution is filtered, degassed, and filtered twice before being extruded from a spinneret; the liquid crystal spinning solution is extruded from the spinneret and then enters a low-temperature coagulation bath for coagulation and molding, the temperature of the low-temperature coagulation bath is 2-6°C, a skin-core structure is formed in the low-temperature coagulation bath to enhance the fiber strength, and then a high-strength para-aramid fiber is obtained through post-treatment; PPTA polymers with particle sizes ranging from <420 μm and >840 μm are mixed and dissolved using concentrated sulfuric acid at a dissolution temperature of 87-88°C for a dissolution time of 1.5-2.0 h to form a spinning solution with a concentration of 19.5-20.5%; wherein the mass ratio of the PPTA polymer with a particle size range of <420 μm to the PPTA polymer with a particle size range of >840 μm is (1-4):1; the spinning solution is degassed and filtered, and then extruded from a spinneret; after being extruded from the spinneret, the spinning solution enters a high-temperature coagulation bath for coagulation and molding; the coagulation bath temperature is 21-27°C; and then post-processed to obtain high-elongation para-aramid fiber.
2. The method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer according to claim 1, characterized in that: The IV value of the PPTA polymer raw material is 5.5-7.5 dL / g, and the test medium for the IV value of the PPTA polymer raw material is concentrated sulfuric acid, the dissolution temperature is 80°C, and the test temperature is 30°C.
3. The method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer according to claim 1, characterized in that: The liquid crystal spinning stock solution is initially filtered through a 15-20 μm sintered felt filter, and after filtration, the liquid crystal spinning stock solution is vacuum degassed through a degassing tower, and then secondary filtered through a 3-8 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement to prepare high-strength para-aramid fiber.
4. The method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer according to claim 1, characterized in that: The spinning solution is vacuum degassed in a degassing tower, filtered through a 3-10 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement to prepare high-elongation para-aramid fiber.
5. The method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer according to claim 1, characterized in that: The waste stock solution slurry and waste silk generated in the process of preparing the high-strength para-aramid fiber and the high-elongation para-aramid fiber are redissolved in concentrated sulfuric acid to form a low-concentration stock solution with a mass concentration of 5-10%, and then the PPTA polymer raw material before screening is added to the low-concentration stock solution to obtain a liquid crystal spinning stock solution with a mass concentration of 19.5-20.4%. After the liquid crystal spinning stock solution is degassed and filtered, it is extruded from a spinneret and coagulated to obtain a common para-aramid fiber; the common para-aramid fiber has a single fiber fineness of 1D-2D and a multi-filament fineness of 200D-2000D; the tensile strength of the common para-aramid fiber is ≥18 cN·dtex -1 , the elongation at break is 3.5±1.0%, and the modulus is 85±20 GPa.
6. The method for preparing para-aramid fiber by comprehensive utilization of PPTA polymer according to claim 5, characterized in that: When the waste stock solution slurry and waste silk are dissolved in concentrated sulfuric acid, the dissolution temperature is 90-95° C. and the dissolution time is 2-2.5 h; The liquid crystal spinning stock solution is vacuum degassed in a degassing tower, filtered through a 5-8 μm sintered felt, and then transported to each spinning position through a split pipeline arrangement; the liquid crystal spinning stock solution is extruded from a spinneret and then enters a coagulation bath for forming, the coagulation bath temperature is 5-8°C, and then post-processed to obtain ordinary para-aramid fiber.