A low-temperature conductive slurry with high electrical performance and its application
By using a low-temperature conductive paste combined with a polyepoxy-thiazole bromine salt conductive organic carrier and micro-nano powder, the problem of high volume resistivity of the low-temperature cured silver paste electrode is solved, the electrical performance and efficiency of HJT solar cells are improved, and the electrical performance and efficiency of HJT solar cells are reduced. cost.
Patent Information
- Application Number
- CN202411126970.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Low-temperature cured silver paste leads to a high volume resistivity in the electrode preparation of HJT solar cells, increasing costs and affecting power generation efficiency. The performance improvement of traditional low-temperature conductive silver paste is limited and cannot match the cost.
Polyepoxy-thiazole bromine salt conductive organic carrier is used to replace traditional binders and combine them with micro-nano powders and additives to prepare low-temperature conductive paste, reducing silver content and improving electrical properties.
It significantly improves the electrical performance of the slurry, reduces body resistance, increases the efficiency of the battery cell, reduces costs, while maintaining stability and printing.
Smart Images

Figure CN118645285B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a low-temperature conductive slurry with high electrical performance and application thereof. Background Art
[0002] Low-temperature curing silver paste is widely used in low-temperature processing of special devices, such as mold attachment of wide-bandgap power devices, circuit printing of flexible electronic devices, perovskite devices, screen printing of heterojunction (SHJ / HJT) solar cells, etc. Due to the good passivation contact structure of hydrogenated amorphous silicon (a-Si:H) film, HJT solar cells are one of the promising materials for the next generation of silicon-based solar cells. The H atoms in a-Si:H film can passivate the dangling bonds of silicon, and its content determines the optoelectronic properties of HJT solar cells. However, the H atoms in a-Si:H film have a great influence on the processing temperature. Therefore, compared with traditional high-temperature sintered silicon solar cells, SHJ solar cells require low-temperature metallization. At present, the metallization of industrial HJT solar cells is mainly achieved by screen printing low-temperature curing silver paste. However, the volume resistivity of the electrode prepared by low-temperature curing silver paste is 2-3 times higher than that of the electrode prepared by high-temperature sintering silver paste. This is because the organic phase curing of low-temperature silver paste will fully wrap the powder, thereby increasing the resistivity. In order to achieve effective current collection, more silver paste is consumed on the electrodes of HJT cells. In addition, the price of low-temperature curing silver paste is generally higher than that of high-temperature sintering silver paste. These factors increase the cost of screen printing and weaken the competitiveness of HJT solar cells as the next generation of silicon-based solar cells.
[0003] The research on low-temperature conductive silver paste mainly includes the surface treatment of conductive phase particles, the doping of organic phase phenolic resin and the addition of various additives. In these two aspects of research, the performance improvement of conductive silver paste is still unsatisfactory, mainly because the organic phase phenolic resin is not conductive, and the cured resin has been fully coated on the surface of the conductive phase particles, which hinders the transmission of electrons and makes the body resistance of the electrode too large, thereby affecting the power generation efficiency of solar cells. Even if the overall silver content of the paste is increased unilaterally to improve its electrical properties, the improved electrical performance cannot match the rising costs.
[0004] The present invention adopts polyepoxy-thiazole bromide conductive organic carrier to replace traditional adhesives such as epoxy resin and phenolic resin, mixes with powder in different proportions and adds various additives to prepare low-temperature conductive slurry samples. The silver content of the slurry is reduced, the electrical properties of the slurry are greatly improved, and the demand for cost reduction and efficiency improvement is achieved. Summary of the invention
[0005] In order to meet the requirements of solar cells for cost reduction and efficiency improvement, the object of the present invention is to provide a low-temperature conductive paste with high electrical performance and its application, wherein the low-temperature conductive paste has excellent electrical properties, stable printability and good durability.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is:
[0007] A low-temperature conductive paste with high electrical performance, based on the total mass of the conductive paste as 100%, the low-temperature silver paste comprises the following components:
[0008] Organic binder 2%-2.8%;
[0009] Solvent 2%-3.5%;
[0010] Micro-nano powder 88%-94%;
[0011] Additives 0.5%-3.5%;
[0012] The organic binder is a mixture of polyepoxy-thiazole bromide salt conductive organic body and resin, and the auxiliary agent includes a sintering auxiliary agent, which is an organic acid completely dissolved in a solvent.
[0013] Furthermore, the sintering aid includes a combination of one or more of phthalic acid, octanoic acid, oleic acid, benzoic acid, ricinoleic acid, dodecyl mercaptan, and aniline.
[0014] Furthermore, the micro-nano powder includes a combination of one or more of micro-nano spherical silver powder, micro-nano flaky silver powder, micro-nano flaky silver-coated copper powder and micro-nano silver-coated copper powder.
[0015] Furthermore, the specific surface area of the micro-nano spherical silver powder is 1-2.5 m 2 / g, D50 is 0.5-2 microns; the specific surface area of the micro-nano flaky silver powder is 0.2-1 m 2 / g, D50 is 0.5-3 microns; the specific surface area of the micro-nano silver-coated copper powder is 0.15-0.4 m 2 / g, D50 is 0.5-5 microns.
[0016] Furthermore, the auxiliary agent also includes a combination of one or more of a latent curing agent, a leveling agent, a dispersant, and a defoaming agent.
[0017] Furthermore, the solvent includes any one or more combinations of terpineol, diethyl succinate, diethylene glycol monoethyl ether acetate, CZ-12, dipropylene glycol methyl ether, N-methyl pyrrolidone, dimethyl maleate, and diethylene glycol butyl ether acetate.
[0018] Furthermore, the leveling agent includes any one of polydimethylsiloxane, polyether polyester modified organic siloxane, butyl cellulose, polyacrylic acid, and turpentine, or a combination of at least two thereof.
[0019] Furthermore, the dispersant and defoamer include any one of oleic acid, stearic acid, ethyl acetoacetate, butyrylacetone, polyethylene glycol, hydrogenated castor oil, and polyamide wax, or a combination of at least two thereof.
[0020] Furthermore, the resin is an epoxy resin with an average molecular weight of 100-10000, and the synthesis steps of the polyepoxy-thiazole bromide conductive organic body are: dissolving polythiazole in a corresponding solvent, using anhydrous AlCl3 as a catalyst, coupling multiple epoxy groups on its thiazole ring to obtain a polyepoxy-thiazole precursor, and the specific preparation formula is:
[0021] Then, the AlCl3 catalyst and other solvents were filtered and removed, the prepolymer was precipitated with an inert solvent, and the unreacted monomers were eluted to obtain a prepolymer with a purity greater than 95%. Finally, benzyl bromide was used as a dopant to introduce negative ions (Cl - ), obtain polyepoxy-thiazole bromide, the specific preparation formula is: .
[0022] Furthermore, an application of a low-temperature conductive paste with high electrical performance is provided, wherein the paste is used for preparing heterojunction solar cells.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the polyepoxy-thiazole bromide polymer used in the present invention replaces part of the epoxy resin, which has a significant improvement effect on the electrical properties of the slurry, greatly improves the short-circuit current and open-circuit voltage of the battery cell, and reduces the loss of FF, body resistance difference and other phenomena.
[0024] The present invention creatively combines polyepoxy-thiazole bromide polymer with low-temperature conductive paste, greatly improving the electrical properties of the paste while maintaining stability, tensile strength, solderability and other properties. Under the electrical performance machine test, the adhesive is changed from the original monoepoxy resin to a mixture of polyepoxy-thiazole bromide and epoxy resin, and the bulk resistance is reduced by 30% compared with the original, while the short-circuit current and open-circuit voltage are increased by 5%, thereby improving the efficiency of a single battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Wire resistance curve of low temperature slurry of Example 1-6;
[0026] Figure 2 is the DSC curing curve of the low temperature slurry of Example 1;
[0027] Figure 3 The solderability of the low temperature paste of Example 1;
[0028] Figure 4 is the DSC curing curve of the low temperature slurry of Comparative Example 1;
[0029] Figure 5 This is the cross-sectional SEM of the low-temperature slurry of Example 1;
[0030] Figure 6 This is the cross-sectional SEM of the low-temperature slurry of Comparative Example 1. DETAILED DESCRIPTION
[0031] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0032] A low-temperature conductive paste with high electrical performance, based on the total mass of the conductive paste as 100%, the low-temperature silver paste comprises the following components:
[0033] Organic binder 2%-2.8%;
[0034] Solvent 2%-3.5%;
[0035] Micro-nano powder 88%-94%;
[0036] Additives 0.5%-3.5%;
[0037] The organic binder is a mixture of polyepoxy-thiazole bromide salt conductive organic body and resin, and the auxiliary agent includes a sintering auxiliary agent, which is an organic acid completely dissolved in a solvent.
[0038] The resin is an epoxy resin with an average molecular weight of 100-10000. The synthesis steps of the polyepoxy-thiazole bromide conductive organic body are: dissolving polythiazole in a corresponding solvent, using anhydrous AlCl3 as a catalyst, coupling multiple epoxy groups on its thiazole ring to obtain a polyepoxy-thiazole precursor. The specific preparation formula is:
[0039] Then, the AlCl3 catalyst and other solvents were filtered and removed, the prepolymer was precipitated with an inert solvent, and the unreacted monomers were eluted to obtain a prepolymer with a purity greater than 95%. Finally, benzyl bromide was used as a dopant to introduce negative ions (Cl - ), obtain polyepoxy-thiazole bromide, the specific preparation formula is: . Example 1
[0040] comprehensive Figure 2As shown, a low-temperature conductive paste for HJT solar cells with high electrical performance comprises, by weight percentage, a particle size of 0.7 microns (D50), a specific surface area of 2.0 m 2 / g of spherical silver powder 20%, particle size 3.0 microns (D50), specific surface area 0.28 m 2 / g of spherical silver-coated copper powder 73%, the silver content of the silver-coated copper powder used is 14%. The adhesive is bisphenol A epoxy resin: polyepoxy-thiazole bromide (1:1) is used in an amount of 3.0%, the molecular weight of bisphenol A epoxy resin is 2000-2300, the amount of imidazole curing agent is 0.5%, the amount of leveling agent polydimethylsiloxane is used in an amount of 0.4%, the amount of polyethylene glycol as a dispersant and defoamer is used in an amount of 0.6%, and the amount of solvent dipropylene glycol methyl ether is used in an amount of 2.5%. First, mix the organic mixture evenly, then add silver powder and silver-coated copper powder, and disperse them evenly with a homogenizer. The resistance of the slurry after printing is 2.37. The same formula uses benzoic acid diglycerol ester type resin instead of polyepoxy-thiazole bromide polymer, and the resistance is 3.44. Example 2
[0041] comprehensive Figure 1 As shown, a low-temperature conductive paste for HJT solar cells with high electrical performance comprises, by weight percentage, a particle size of 0.7 microns (D50), a specific surface area of 2.0 m 2 / g of spherical silver powder 20%, particle size 3.0 microns (D50), specific surface area 0.28 m 2 / g of spherical silver-coated copper powder 73%, the silver content of the silver-coated copper powder used is 14%. The adhesive is polyepoxy-thiazole bromide polymer: bisphenol F type epoxy resin (1:2) dosage is 2.8%, bisphenol F type epoxy resin molecular weight is 1600-1800, the dosage of anhydride curing agent is 0.7%, the dosage of leveling agent polydimethylsiloxane is 0.4%, the dosage of polyethylene glycol as a dispersant and defoamer is 0.6%, and the dosage of solvent dipropylene glycol methyl ether is 2.5%. First, mix the organic mixture evenly, then add silver powder and silver-coated copper powder, and disperse them evenly with a homogenizer. The resistance of the slurry after printing is 2.29. The same formula uses benzoic acid diglycerol ester type resin instead of polyepoxy-thiazole bromide polymer, and the resistance is 3.56. Example 3
[0042] A low-temperature conductive paste for HJT solar cells with high electrical performance, the composition of which, calculated by mass percentage, includes: a particle size of 0.49 microns (D50), a specific surface area of 2.4 m 2 / g of spherical silver powder 30%, particle size 3.5 microns (D50), specific surface area 0.25 m 2 / g of spherical silver-coated copper powder 62%, the silver content of the silver-coated copper powder used is 8%. The adhesive is o-cresol formaldehyde epoxy resin: polyepoxy-thiazole bromide (1:1) with a dosage of 3.8%, o-cresol formaldehyde epoxy resin molecular weight of 5600-5700, imidazole curing agent dosage of 0.7%, leveling agent polydimethylsiloxane dosage of 0.6%, polyamide wax as dispersant and defoamer dosage of 0.5%, solvent dipropylene glycol methyl ether dosage of 2.5%. First, mix the organic thoroughly, then add silver powder and silver-coated copper powder, and disperse them evenly with a homogenizer. The resistance of the slurry after printing is 3.1. The same formula uses benzoic acid diglycerol ester type resin instead of polyepoxy-thiazole bromide polymer, and the resistance is 4.37. Example 4
[0043] A low-temperature conductive paste for HJT solar cells with high electrical performance, the composition of which, calculated by mass percentage, includes: a particle size of 0.5 microns (D50), a specific surface area of 2.6 m 2 / g of spherical silver powder 41%, particle size 5.1 microns (D50), specific surface area of 0.5 m 2 / g of blocky silver-coated copper powder 52%, the silver content of the silver-coated copper powder used is 12%. Linear phenolic polycondensate resin: polyepoxy-thiazole bromide (1:1) dosage is 2.8%, the molecular weight of o-cresol formaldehyde epoxy resin is 5600-5700, the dosage of boron amine curing agent is 0.6%, the dosage of leveling agent turpentine is 0.4%, the dosage of polyethylene glycol as dispersant and defoamer is 0.6%, and the dosage of solvent dipropylene glycol methyl ether is 2.6%. First, mix the organic mixture evenly, then add silver powder and silver-coated copper powder, and disperse them evenly with a homogenizer. The resistance of the slurry after printing is 2.77. The same formula uses benzoic acid diglycerol ester type resin instead of polyepoxy-thiazole bromide polymer, and the resistance is 4.1. Example 5
[0044] comprehensive Figure 3-4 As shown, a low-temperature conductive paste for HJT solar cells with high electrical performance comprises, by weight percentage, a particle size of 0.4 μm (D50), a specific surface area of 2.9 m 2 / g of spherical silver powder 37%, particle size 3.5 microns (D50), specific surface area of 0.50 m 2 / g of flaky silver powder 9%, particle size 3.8 microns (D50), specific surface area 0.26m 2 / g of spherical silver-coated copper powder 46%, the silver content of the silver-coated copper powder used is 16%. Polyether epoxy resin: polyepoxy-thiazole bromide (1:2) dosage is 3%, polyether epoxy resin molecular weight is 900-1000, boron amine curing agent dosage is 0.8%, leveling agent polydimethylsiloxane dosage is 0.5%, stearic acid dosage as dispersant and defoamer is 1%, solvent dipropylene glycol methyl ether dosage is 2.7%. First mix the organic mixture evenly, then add silver powder and silver-coated copper powder, and disperse evenly with a homogenizer. The resistance of the slurry after printing is 2.85. The same formula uses benzoic acid diglycerol ester type resin instead of polyepoxy-thiazole bromide polymer, and the resistance is 4.06. Example 6
[0045] A low-temperature conductive paste for HJT solar cells with high electrical performance, the composition of which, calculated by mass percentage, includes: a particle size of 0.5 microns (D50), a specific surface area of 2.7 m 2 / g of spherical silver powder 30.5%, particle size 1.9 microns (D50), specific surface area 0.72 m 2 / g of flaky silver powder 62%. Glycerol epoxy resin: polyepoxy-thiazole bromide (1:1) dosage is 3%, glycerol epoxy resin molecular weight is 600-800, imidazole curing agent dosage is 0.7%, leveling agent polydimethylsiloxane dosage is 0.7%, stearic acid and polyethylene glycol (1:1) dosage as dispersant and defoamer is 0.6%, solvent dipropylene glycol methyl ether dosage is 2.5%. First mix the organic mixture evenly, then add silver powder and silver-coated copper powder, and disperse evenly with a homogenizer. The resistance of the slurry after printing is 1.79. The same formula uses benzoic acid diglycerol ester type resin instead of polyepoxy-thiazole bromide polymer, and the resistance is 2.27.
[0046] Comparative Examples 1-6
[0047] The market's leading low-temperature conductive silver-clad copper paste.
[0048] Specific slurries include:
[0049] Comparative Example 1: Crystal Silver HAC549;
[0050] Comparative Example 2: KE132 from Japan KE Company;
[0051] Comparative Example 3: Crystal Silver HAC569-T6S7;
[0052] Comparative Example 4: Xinghan AC-301-G16;
[0053] Comparative Example 5: Xinghan AC-101-A11;
[0054] Comparative Example 6: Xinghan AC-101-A15.
[0055] The above slurries were tested for performance
[0056] Paste resistance test: After printing the same batch, dry and cure under the same conditions, and test the resistance with a Keithley source meter.
[0057] Total wet weight test of front and back auxiliary materials: Use the difference method to test the weight change of a single piece before and after printing, measure 5 pieces and take the average value.
[0058] Photoelectric conversion efficiency test: The photoelectric conversion efficiency is measured by Maxwell's HJT screen printing equipment. 20 pieces are measured and the average value is taken.
[0059]
[0060] According to the comparison between the embodiments and the comparative examples, the high electrical performance HJT solar cell low-temperature conductive paste provided by the present invention changes the adhesive from the original monoepoxy resin to a mixture of polyepoxy-thiazole bromide and epoxy resin, and the body resistance is reduced by 30% compared with the original. Under the premise of maintaining stability, the wet weight is 3 to 5 mg lower than that of ordinary solvents. In addition, the efficiency of the battery cell is improved by serial welding to make components.
[0061] The above description is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiment. Any equivalent modifications or changes made by ordinary technicians in this field based on the contents disclosed by the present invention should be included in the protection scope recorded in the claims.
Claims
1. A low-temperature conductive paste with high electrical performance, characterized in that: Taking the total mass of the conductive paste as 100%, the conductive paste includes the following components: Organic binder 2%-2.8%; Solvent 2%-3.5%; Micro-nano powder 88%-94%; Additives 0.5%-3.5%; The organic binder is a mixture of polyepoxy-thiazole bromide conductive organic body and resin, and the auxiliary agent includes a sintering aid, which is an organic acid completely dissolved in the solvent; The synthesis steps of the polyepoxy-thiazole bromide conductive organic body are as follows: dissolving polythiazole in a corresponding solvent, using anhydrous AlCl3 as a catalyst, coupling multiple epoxy groups on its thiazole ring to obtain a polyepoxy-thiazole precursor. The specific preparation formula is: Then, the AlCl3 catalyst and other solvents are filtered and removed, the prepolymer is precipitated with an inert solvent, and the unreacted monomer is eluted to obtain a prepolymer with a purity greater than 95%. Finally, benzyl bromide is used as a dopant to introduce negative ions to obtain polyepoxy-thiazole bromide. The specific preparation formula is: 。 2. The low-temperature conductive paste with high electrical performance according to claim 1, characterized in that: The sintering aid includes one or more of phthalic acid, octanoic acid, oleic acid, benzoic acid, ricinoleic acid, dodecyl mercaptan and aniline.
3. The low-temperature conductive paste with high electrical performance according to claim 1, characterized in that: The micro-nano powder includes a combination of one or more of micro-nano spherical silver powder, micro-nano flaky silver powder and micro-nano silver-coated copper powder.
4. The low-temperature conductive paste with high electrical performance according to claim 3, characterized in that: The specific surface area of the micro-nano spherical silver powder is 1-2.5 m 2 / g, D50 is 0.5-2 microns; the specific surface area of the micro-nano flaky silver powder is 0.2-1 m 2 / g, D50 is 0.5-3 microns; the specific surface area of the micro-nano silver-coated copper powder is 0.15-0.4 m 2 / g, D50 is 0.5-5 microns.
5. The low-temperature conductive paste with high electrical performance according to claim 1, characterized in that: The auxiliary agent also includes a combination of one or more of a latent curing agent, a leveling agent, a dispersant, and a defoaming agent.
6. The low-temperature conductive paste with high electrical performance according to claim 5, characterized in that: The solvent includes any one or more combinations of terpineol, diethyl succinate, diethylene glycol monoethyl ether acetate, alcohol ester dodecasol, dipropylene glycol methyl ether, N-methyl pyrrolidone, dimethyl maleate, and diethylene glycol butyl ether acetate.
7. The low-temperature conductive paste with high electrical performance according to claim 5, characterized in that: The leveling agent includes any one of polydimethylsiloxane, polyether polyester modified organic siloxane, butyl cellulose, polyacrylic acid, and turpentine, or a combination of at least two of them.
8. The low-temperature conductive paste with high electrical performance according to claim 5, characterized in that: The dispersant and defoamer include any one of oleic acid, stearic acid, ethyl acetoacetate, butyrylacetone, polyethylene glycol, hydrogenated castor oil, and polyamide wax, or a combination of at least two thereof.
9. The low-temperature conductive paste with high electrical performance according to claim 2, characterized in that: The resin is an epoxy resin with an average molecular weight of 100-10000.
10. An application of the low-temperature conductive paste with high electrical performance according to any one of claims 1 to 9, characterized in that: The slurry is used for preparing heterojunction solar cells.