Ultraviolet light curing material, curing polymer material, preparation method and application thereof

By using disulfide five-membered ring monomers in ultraviolet cured materials, polymers with disulfide bonds, peptide bonds and multiple hydrogen bonds are solved, and the problem of difficult balance of hardness and toughness of traditional ultraviolet cured materials is achieved. Hardness and high toughness polymer materials have expanded their application range.

CN118652428BActive Publication Date: 2024-11-19ZHEJIANG MINSTER NEW MATERIALS CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202411097080.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-19
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Traditional ultraviolet curing materials are difficult to balance hardness and toughness after curing, resulting in poor toughness and easy brittle cracking, which limits their application areas.

Method used

A disulfide five-membered ring monomer is used as the ultraviolet curing material to generate a polymer with disulfide bonds, peptide bonds and multiple hydrogen bonds through photocuring reactions, ensuring that the material has high hardness and high toughness after curing.

Benefits of technology

It has achieved excellent hardness, toughness and chemical stability of the cured polymer material, reduced the cost of reagents, improved the biocompatibility and scope of application, and expanded the application prospects in the fields of drug delivery, biomaterials, etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652428B_ABST
    Figure CN118652428B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of ultraviolet light-curing materials, and specifically relates to ultraviolet light-curing materials, cured polymer materials, preparation methods and applications thereof. The ultraviolet light-curing materials include disulfide five-membered ring monomers. When the ultraviolet light-curing materials are exposed to ultraviolet light, the disulfide bonds in the disulfide five-membered rings are opened and polymerization occurs to generate cured polymer materials. The present invention provides disulfide five-membered ring monomers with unique chemical structures by rationally designing and optimizing the monomer structure of ultraviolet light-curing materials. In the disulfide five-membered ring monomers, peptide bonds and / or multiple hydrogen bonds can induce the orderly arrangement of the disulfide five-membered ring monomers, so that the disulfide bonds in the disulfide five-membered ring monomers are opened, and polymerization occurs rapidly under ultraviolet light irradiation to generate disulfide bond-based polymers. Under the joint action of multiple hydrogen bonds and / or disulfide bonds in the disulfide five-membered ring monomers, the prepared cured polymer material has excellent hardness, toughness and chemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultraviolet light curing materials, and in particular to ultraviolet light curing materials, curing polymer materials, and preparation methods and applications thereof. Background Art

[0002] UV curing materials have shown excellent application prospects in many fields such as coatings, adhesives, printing inks, etc. due to their unique curing mechanism. Compared with traditional thermal curing materials or solvent evaporation materials, UV curing materials have significant advantages, including but not limited to:

[0003] 1. Rapid curing: UV curing technology can achieve a curing speed of seconds to minutes, greatly improving production efficiency and meeting the needs of modern automatic production lines for rapid processing.

[0004] 2. Environmentally friendly: UV-curable materials release almost no volatile organic compounds during the curing process, which can significantly reduce pollution to the environment.

[0005] 3. Low energy consumption: Compared with the thermal curing process in the existing technology, UV curing materials do not require additional heating during the curing process, the energy required is significantly reduced, and the production cost can be reduced.

[0006] However, despite its many advantages, the polymer materials obtained after curing of traditional UV-curable materials still have the problem of difficult balance between hardness and toughness. Specifically, UV-curable materials often show higher hardness and wear resistance after curing, which is due to their highly cross-linked structure, which helps to improve the scratch resistance and chemical stability of the material. However, at the same time, this high degree of cross-linking also leads to poor toughness of UV-curable materials after curing, and they are prone to brittle cracking, especially at low temperatures or under repeated stress. The impact resistance and ductility of polymer materials are limited, which limits their application areas. For example, in the field of coatings, although the high-hardness polymer materials obtained after curing UV-curable materials can provide excellent surface protection, the brittleness of the material may cause cracking during long-term use, reducing the durability and aesthetics of the coating.

[0007] Therefore, it is necessary to provide a UV-curable material in which the polymer material obtained after curing has both high hardness and high toughness. Summary of the invention

[0008] 1. Technical issues to be resolved

[0009] In view of the above technical problems, the present invention provides a UV-curable material, a cured polymer material, a preparation method and application thereof, so that the polymer material obtained after the high UV-curable material is cured has both high hardness and toughness.

[0010] (II) Technical solution

[0011] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0012] In a first aspect, the present invention provides a UV-curable material, comprising a disulfide five-membered ring monomer, wherein the disulfide five-membered ring monomer has a general structural formula of:

[0013] ;

[0014] Wherein, the specific structural formula of the R group is any one of the following:

[0015] .

[0016] In a second aspect, the present invention provides a use of the above-mentioned UV-curable material in UV-curable coatings, UV-curable printing inks or UV-curable adhesives.

[0017] In a third aspect, the present invention provides a use of the above-mentioned UV curable material in the preparation of a cured polymer material.

[0018] In a fourth aspect, the present invention provides a solidified polymer material, wherein the solidified polymer material has the general structural formula:

[0019] ;

[0020] In the above general structural formula, the specific structural formula of the R group is any one of the following:

[0021] ;

[0022] In the above general structural formula, the value of n is 100-2000.

[0023] In a fifth aspect, the present invention provides a method for preparing the above-mentioned cured polymer material, which specifically comprises: using the above-mentioned ultraviolet light-curing material as a polymerization precursor, performing a photocuring reaction, and preparing a cured polymer material.

[0024] In the method for preparing the cured polymer material as described above, preferably, the photocuring reaction is carried out under the condition of ultraviolet light irradiation.

[0025] In the method for preparing the cured polymer material as described above, preferably, the central wavelength of the ultraviolet light is 365±5nm, and the radiation intensity of the ultraviolet light is 80-120w / cm 2 The UV irradiation time is 5-40s.

[0026] In the method for preparing the cured polymer material as described above, preferably, the temperature of the photocuring reaction is 15-30°C.

[0027] In a sixth aspect, the present invention further provides the use of the above-mentioned solidified polymer material or the solidified polymer material prepared by the above-mentioned preparation method in drug delivery materials, drug delivery carriers, biomaterials or biosensors.

[0028] (III) Beneficial effects

[0029] The present invention provides a disulfide five-membered ring monomer with a unique chemical structure by rationally designing and optimizing the monomer structure of the ultraviolet curing material. In the disulfide five-membered ring monomer, peptide bonds and / or multiple hydrogen bonds can induce the disulfide five-membered ring monomer to be arranged in an orderly manner, so that the disulfide bonds in the disulfide five-membered ring monomer are opened, and a polymerization reaction occurs rapidly under ultraviolet light irradiation to generate a disulfide bond-based polymer. Under the joint action of the multiple hydrogen bonds and / or disulfide bonds in the disulfide five-membered ring monomer, the prepared cured polymer material has excellent hardness, toughness and chemical stability.

[0030] In the present invention, the photocuring reaction of the UV-curable material can be carried out under light conditions only, without adding a photoinitiator or a photosensitizer to the monomer. On the one hand, it can reduce the reagent cost, and on the other hand, it can effectively ensure the purity of the prepared cured polymer material, thereby improving the biocompatibility and application range of the polymer material.

[0031] In addition, disulfide bonds, peptide bonds and multiple hydrogen bonds can also give the cured polymer materials good biocompatibility and degradability, making them have broad application prospects in the fields of drug delivery materials, drug delivery carriers, biomaterials and biosensors. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The schematic diagram of the reaction of preparing a cured polymer material by using an ultraviolet curing material in the present invention;

[0033] Figure 2 The nuclear magnetic resonance hydrogen spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 1;

[0034] Figure 3 The Raman spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 1;

[0035] Figure 4 The DSC graph of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 1;

[0036] Figure 5 is a stress-strain curve diagram of the cured polymer material prepared in Example 1;

[0037] Figure 6The nuclear magnetic resonance hydrogen spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 2;

[0038] Figure 7 The Raman spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 2;

[0039] Figure 8 The DSC graph of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 2;

[0040] Fig. 9 is a stress-strain curve diagram of the cured polymer material prepared in Example 2;

[0041] Fig.10 The nuclear magnetic resonance hydrogen spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 3;

[0042] Fig.11 The Raman spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 3;

[0043] Fig.12 The DSC graph of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 3;

[0044] Fig.13 This is a stress-strain curve of the cured polymer material prepared in Example 3;

[0045] Fig.14 is the hydrogen nuclear magnetic resonance spectrum of the disulfide five-membered ring monomer in Example 4;

[0046] Fig.15 The Raman spectra of the disulfide five-membered ring monomer and the prepared cured polymer material in Example 4;

[0047] Fig.16 This is a stress-strain curve of the cured polymer material prepared in Example 4. DETAILED DESCRIPTION

[0048] In order to better explain the present invention and facilitate understanding, the present invention is described in detail with reference to the accompanying drawings and specific implementation methods below.

[0049] The present invention provides an ultraviolet curing material, comprising a disulfide five-membered ring monomer. The general structural formula of the disulfide five-membered ring monomer in the present invention is:

[0050] .

[0051] The specific structural formula of the R group can be any of the following:

[0052] .

[0053] The present invention also provides an application of the ultraviolet curing material in ultraviolet curing coating, ultraviolet curing printing ink or ultraviolet curing adhesive.

[0054] In addition, the present invention also provides a use of the above-mentioned ultraviolet curing material in preparing a curing polymer material.

[0055] In addition, the present invention also provides a solidified polymer material, the general structural formula of the solidified polymer material is:

[0056] .

[0057] In the above general structural formula, the specific structural formula of the R group is any one of the following:

[0058] .

[0059] In the above general structural formula, the value of n can be 100-2000.

[0060] like Figure 1 As shown, the preparation method of the above-mentioned cured polymer material includes: using the above-mentioned ultraviolet light curing material as a polymerization precursor, making it undergo a photocuring reaction under ultraviolet light irradiation conditions, and preparing a cured polymer material. Preferably, in the photocuring reaction, the central wavelength of the ultraviolet light is 365±5nm, and the radiation intensity of the ultraviolet light is 80-120w / cm 2 The UV irradiation time is 5-40s, and the temperature of the photocuring reaction is 15-30℃.

[0061] In the present invention, the radiation intensity of the ultraviolet light and the time of ultraviolet light irradiation need to be maintained within the above range to ensure that the cured polymer material has both high hardness and toughness. If the radiation intensity of the ultraviolet light and the time of ultraviolet light irradiation are greater than the above range, the toughness of the cured polymer material will decrease.

[0062] In the disulfide five-membered ring monomer of the present invention, the R group can be connected to the carbon No. 1 in the disulfide five-membered ring, or can be connected to the carbon No. 2 in the disulfide five-membered ring. Moreover, it has been verified through experiments that for the same R group, whether the R group is connected to the carbon No. 1 or the carbon No. 2 in the disulfide five-membered ring, the hardness and toughness of the cured polymer material prepared through the photocuring reaction are almost the same.

[0063] In the present invention, the photocuring reaction of the UV-curable material can be carried out under light conditions only, without adding a photoinitiator or a photosensitizer to the monomer. On the one hand, it can reduce the reagent cost, and on the other hand, it can effectively ensure the purity of the prepared cured polymer material, thereby improving the biocompatibility and application range of the polymer material.

[0064] In addition, the present invention also provides the use of the above-mentioned solidified polymer material or the solidified polymer material prepared by the above-mentioned preparation method in drug delivery materials, drug delivery carriers, biomaterials or biosensors.

[0065] The present invention provides a disulfide five-membered ring monomer with a unique chemical structure by rationally designing and optimizing the monomer structure of the ultraviolet curing material. In the disulfide five-membered ring monomer of the present invention, peptide bonds and / or multiple hydrogen bonds can induce the disulfide five-membered ring monomer to be arranged in an orderly manner, so that the disulfide bonds in the disulfide five-membered ring monomer are opened, and a polymerization reaction occurs rapidly under ultraviolet light irradiation to generate a disulfide bond-based polymer. Under the combined action of the multiple hydrogen bonds and / or disulfide bonds in the disulfide five-membered ring monomer, the prepared cured polymer material has excellent hardness, toughness and chemical stability. In the prior art, the elongation, i.e., toughness, of the cured polymer material prepared by the ultraviolet curing material is generally less than 10%, while the tensile properties of the cured polymer material prepared by the ultraviolet curing material of the present invention range from 11 to 156%.

[0066] In addition, the disulfide bonds, peptide bonds and multiple hydrogen bonds in the disulfide five-membered ring monomer can also give the cured polymer material good biocompatibility and degradability, making it have broad application prospects in the fields of drug delivery, biomaterials and biosensors.

[0067] In order to further clarify the scheme of the present invention and its technical advancement, the following is a description in conjunction with specific embodiments and technical effects.

[0068] Example 1

[0069] This embodiment provides a method for preparing a cured polymer material, comprising the following steps: placing a disulfide five-membered ring monomer (monomer 1) under ultraviolet light for photocuring reaction to prepare a cured polymer material (polymer 1). Specifically, the central wavelength of the ultraviolet light is 365nm, and the radiation intensity of the ultraviolet light is 100w / cm 2 , the UV irradiation time is 25s, and the temperature of the photocuring reaction is 20℃.

[0070] The disulfide five-membered ring monomer in this embodiment is:

[0071] .

[0072] In this embodiment, the reaction principle of curing the polymer material is as follows:

[0073] .

[0074] Figure 2 is the nuclear magnetic resonance hydrogen spectrum of the disulfide five-membered ring monomer and the cured polymer material in this embodiment, Figure 3 The Raman spectra of the disulfide five-membered ring monomer and the cured polymer material in this embodiment are shown in FIG. Figure 3 It can be seen that the SS vibration peak of the five-membered ring in the disulfide five-membered ring monomer structure in this embodiment is 506 cm -1 , which is transformed into the vibration peak 506cm of the chain hydrocarbon SS in the solidified polymer material -1 and 520cm -1 , Figure 4 The DSC diagram of the disulfide five-membered ring monomer and the cured polymer material in this embodiment is shown in FIG. Figure 4 It can be seen that after the disulfide five-membered ring monomer is polymerized into a solidified polymer material, the melting point disappears.

[0075] The mechanical properties of the cured polymer material prepared in this example were tested, and the results were as follows: Figure 5 ,pass Figure 5 It can be seen that the tensile strength of the cured polymer material prepared in this embodiment is 30.7 MPa, and the elongation is 16%.

[0076] Example 2

[0077] This embodiment provides a method for preparing a cured polymer material, comprising the following steps: placing a disulfide five-membered ring monomer (monomer 2) under ultraviolet light for photocuring reaction to prepare a cured polymer material (polymer 2). Specifically, the central wavelength of the ultraviolet light is 370nm, and the radiation intensity of the ultraviolet light is 80w / cm 2 The UV irradiation time is 40s and the photocuring reaction temperature is 15°C.

[0078] The disulfide five-membered ring monomer in this embodiment is:

[0079] .

[0080] In this embodiment, the reaction principle of curing the polymer material is as follows:

[0081] .

[0082] Figure 6 is the nuclear magnetic resonance hydrogen spectrum of the disulfide five-membered ring monomer and the cured polymer material in this embodiment, Figure 7 The Raman spectra of the disulfide five-membered ring monomer and the cured polymer material in this embodiment are shown in FIG. Figure 7It can be seen that the SS vibration peak of the five-membered ring in the disulfide five-membered ring monomer structure in this embodiment is 506 cm -1 , which is transformed into the vibration peak 506cm of the chain hydrocarbon SS in the solidified polymer material -1 and 520cm -1 , Figure 8 The DSC diagram of the disulfide five-membered ring monomer and the cured polymer material in this embodiment is shown in FIG. Figure 8 It can be seen that after the disulfide five-membered ring monomer is polymerized into a solidified polymer material, the melting point disappears.

[0083] The mechanical properties of the cured polymer material prepared in this example were tested, and the results were as follows: Fig. 9 ,pass Fig. 9 It can be seen that the tensile strength of the cured polymer material prepared in this embodiment is 40 MPa, and the elongation is 11%.

[0084] Example 3

[0085] This embodiment provides a method for preparing a cured polymer material, comprising the following steps: placing a disulfide five-membered ring monomer (monomer 3) under ultraviolet light for photocuring reaction to prepare a cured polymer material (polymer 3). Specifically, the central wavelength of the ultraviolet light is 360nm, and the radiation intensity of the ultraviolet light is 120w / cm 2 , the UV irradiation time is 5s, and the temperature of the photocuring reaction is 30℃.

[0086] The disulfide five-membered ring monomer in this embodiment is:

[0087] .

[0088] In this embodiment, the reaction principle of curing the polymer material is as follows:

[0089] .

[0090] Fig.10 is the nuclear magnetic resonance hydrogen spectrum of the disulfide five-membered ring monomer and the cured polymer material in this embodiment, Fig.11 The Raman spectra of the disulfide five-membered ring monomer and the cured polymer material in this embodiment are shown in FIG. Fig.11 It can be seen that the SS vibration peak of the five-membered ring in the disulfide five-membered ring monomer structure in this embodiment is 508 cm -1 , which is transformed into the vibration peak 503cm of the chain hydrocarbon SS in the solidified polymer material -1 and 522cm -1 , Fig.12 The DSC diagram of the disulfide five-membered ring monomer and the cured polymer material in this embodiment is shown in FIG. Fig.12It can be seen that after the disulfide five-membered ring monomer is polymerized into a solidified polymer material, the melting point disappears.

[0091] The mechanical properties of the cured polymer material prepared in this example were tested, and the results were as follows: Fig.13 ,pass Fig.13 It can be seen that the tensile strength of the cured polymer material prepared in this embodiment is 30.7 MPa, and the elongation is 156%.

[0092] Example 4

[0093] This embodiment provides a method for preparing a cured polymer material, comprising the following steps: placing a disulfide five-membered ring monomer (monomer 4) under ultraviolet light for photocuring reaction to prepare a cured polymer material (polymer 4). Specifically, the central wavelength of the ultraviolet light is 365nm, and the radiation intensity of the ultraviolet light is 90w / cm 2 The UV irradiation time is 30s and the temperature of the photocuring reaction is 25°C.

[0094] The disulfide five-membered ring monomer in this embodiment is:

[0095] .

[0096] In this embodiment, the reaction principle of curing the polymer material is as follows:

[0097] .

[0098] Fig.14 is the hydrogen nuclear magnetic resonance spectrum of the disulfide five-membered ring monomer in this example, Fig.15 The Raman spectra of the disulfide five-membered ring monomer and the cured polymer material in this embodiment are shown in FIG. Fig.15 It can be seen that the SS vibration peak of the five-membered ring in the disulfide five-membered ring monomer structure in this embodiment is 500 cm -1 , which is transformed into the vibration peak 503cm of the chain hydrocarbon SS in the solidified polymer material -1 and 522cm -1 .

[0099] The mechanical properties of the cured polymer material prepared in this example were tested, and the results were as follows: Fig.16 ,pass Fig.16 It can be seen that the tensile strength of the cured polymer material prepared in this embodiment is 34.7 MPa, and the elongation is 117%.

[0100] Example 5

[0101] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0102] .

[0103] Among them, the R group is:

[0104] .

[0105] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 1. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 35.5 MPa, and the elongation is 13.7%.

[0106] Example 6

[0107] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0108] .

[0109] Among them, the R group is:

[0110] .

[0111] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 1. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 38.3 Mpa, and the elongation is 15.6%.

[0112] Example 7

[0113] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0114] .

[0115] Among them, the R group is:

[0116] .

[0117] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 2. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 36.8 Mpa, and the elongation is 15%.

[0118] Example 8

[0119] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0120] .

[0121] Among them, the R group is:

[0122] .

[0123] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 2. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 38.8 Mpa, and the elongation is 13.8%.

[0124] Example 9

[0125] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0126] .

[0127] Among them, the R group is:

[0128] .

[0129] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 2. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 39.3 Mpa, and the elongation is 14.2%.

[0130] Example 10

[0131] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0132] .

[0133] Among them, the R group is:

[0134] .

[0135] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 2. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 40Mpa, and the elongation is 14%.

[0136] Embodiment 11

[0137] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0138] .

[0139] Among them, the R group is:

[0140] .

[0141] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 1. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 35.2 Mpa, and the elongation is 120%.

[0142] Example 12

[0143] This embodiment provides a method for preparing a solidified polymer material. The difference from Embodiment 1 is that the general structural formula of the disulfide five-membered ring monomer in this embodiment is:

[0144] .

[0145] Among them, the R group is:

[0146] .

[0147] In the disulfide five-membered ring monomer of this embodiment, the R group is connected to carbon 2. After testing, the tensile strength of the cured polymer material prepared in this embodiment is 33.6 Mpa, and the elongation is 103.4%.

[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cured polymer material, characterized in that: Using ultraviolet light curing material as a polymerization precursor, performing a photocuring reaction, and preparing a cured polymer material; The UV curable material includes a disulfide five-membered ring monomer, and the general structural formula of the disulfide five-membered ring monomer is: ; Wherein, the specific structural formula of the R group is any one of the following: ; The general structural formula of the solidified polymer material is: ; In the above general structural formula, the specific structural formula of the R group is any one of the following: ; In the above structural formula, the value of n is 100-2000; The photocuring reaction is carried out under the condition of ultraviolet light irradiation, the central wavelength of the ultraviolet light is 365±5nm, and the radiation intensity of the ultraviolet light is 80-120w / cm 2 , the UV irradiation time is 5-40s; The photocuring reaction can be carried out only under light conditions, and there is no need to add a photoinitiator or a photosensitizer to the disulfide five-membered ring monomer.

2. The cured polymer material according to claim 1, characterized in that The temperature of the photocuring reaction is 15-30°C.

3. Use of the solidified polymer material according to any one of claims 1 to 2 in a drug delivery material, a drug delivery carrier, a biomaterial or a biosensor.

Citation Information

Patent Citations

  • Uses of dithiolane compounds for the photoprotection of the skin, dithiolane compounds and compositions containing same

    CN101683311A

  • Process for depigmenting keratin materials using dithiolane compounds

    CN101744740A

  • Cosmetic composition and a light stabilizing method thereof

    CN101810543A

  • Preparation method of photo-crosslinking dynamic reversible supramolecular polymer adhesive based on lipoic acid small molecular compound

    CN113061263A

  • Lipoic acid-based hydrogel as well as preparation method and application thereof

    CN114058014A