A fireproof heat-insulating coating material and its preparation process

By combining titanium dioxide, vapor-phase silica, composite Eloshima nanotube hybrids and composite aqueous epoxy emulsions, the water resistance and adhesion problems of fire-resistant and thermal insulation coating materials are solved, and high flame retardant and Water-resistant coating material, suitable for environmentally friendly applications.

CN118652606BActive Publication Date: 2024-12-06NINGBO BLUE CORE MICRO NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411061970.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-12-06
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing environmentally friendly fire-resistant and heat-insulating coating materials have problems such as poor water resistance and poor adhesion of substrates, which hinder their application.

Method used

Using titanium dioxide, vapor-phase silica, composite Eloshi nanotube hybrids, composite aqueous epoxy emulsion, polyamino N-P-Si flame retardant, etc., the reaction of the curing agent is carried out to prepare high fire resistance. Fire-resistant and heat-resistant coating materials for flame retardant and water resistance.

Benefits of technology

It realizes a non-toxic and harmless fire-resistant and heat-resistant coating material that is simple to construct, has high flame retardancy and water resistance, is suitable for human and environmentally friendly, and improves the safety fire resistance and adhesion of coating material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 3OIZZCUE4ISZNRZFSBJDK9Z3XKFWXII23IS31WIL
    Figure 3OIZZCUE4ISZNRZFSBJDK9Z3XKFWXII23IS31WIL
Patent Text Reader

Abstract

The invention relates to the field of fire prevention, in particular to a fireproof and heat-insulating coating material and a preparation process thereof. Molybdenum disulfide is in-situ grown on the surface of a halloysite nanotube to prepare a halloysite nanotube hybrid, dopamine and a silane coupling agent 3-(2,3-epoxypropoxy)propyltrimethoxysilane are used as modifiers to perform double-layer modification on the halloysite nanotube hybrid, and a polyamino-containing N-P-Si flame retardant is grafted by epoxy-amino reaction; citraconic anhydride, itaconic anhydride and polyethylene glycol are used as raw materials, and an environmentally friendly epoxy emulsifier is prepared without adding a catalyst, and then polyethylene glycol containing a hydrophilic ethylene oxide segment is reacted with an epoxy group to introduce a polyethylene oxide segment, and an amino group of the polyamino-containing N-P-Si flame retardant is reacted with an epoxy group to introduce an N-P-Si flame retardant element, and a composite waterborne epoxy emulsion is obtained under the action of the environmentally friendly epoxy emulsifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fire prevention, in particular to a fireproof and heat-insulating coating material and a preparation process thereof. Background Art

[0002] Fireproof and heat-insulating coating material is a relatively special coating material. When applied to various metal equipment and the exterior walls of civil buildings, it plays the role of bonding, protection and fire prevention. It can block the spread of fire in the event of a fire and improve the fire resistance limit of the substrate.

[0003] In recent years, with the promotion of environmental concepts, low-toxic and environmentally friendly fire-proof and heat-insulating coating materials have become the focus of exploration in this field. Most of the existing environmentally friendly fire-proof and heat-insulating coating materials on the market have disadvantages such as poor water resistance and poor adhesion to the substrate, which seriously hinders the application of fire-proof and heat-insulating coating materials. Summary of the invention

[0004] The object of the present invention is to provide a fireproof and heat-insulating coating material and a preparation process thereof, so as to solve the problems in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A preparation process of a fireproof and heat-insulating coating material comprises the following steps:

[0007] S1: adding titanium dioxide, fumed silica, and composite halloysite nanotube hybrid into a stirring tank, stirring and grinding to obtain a slurry;

[0008] S2: Mix the composite water-based epoxy emulsion, the additive and the slurry, add the curing agent, stir and discharge the material to obtain a fireproof and heat-insulating coating material.

[0009] Furthermore, the auxiliary agent is a wetting agent, a dispersing agent, and a defoaming agent compounded in a mass ratio of 2:1:1.

[0010] Furthermore, the curing agent is an amine curing agent.

[0011] Furthermore, the raw material composition of the fireproof and heat-insulating coating material is, by weight: 55-70 parts of composite water-based epoxy emulsion, 1-4 parts of auxiliary agent, 5-12 parts of curing agent, 1-5 parts of titanium dioxide, 2-4 parts of fumed silica, and 6-12 parts of composite halloysite nanotube hybrid.

[0012] Further, the preparation of the composite waterborne epoxy emulsion comprises the following steps:

[0013] 1) Mix citraconic anhydride, itaconic anhydride and polyethylene glycol, heat to 78-82°C and keep warm for 1-2 hours, add epoxy resin E51 and epoxy resin E20, heat to 118-122°C and keep warm for 3-4 hours, cool and obtain an emulsifier;

[0014] 2) Mix epoxy resin E51, epoxy resin E20, dipropylene glycol methyl ether and ethylene glycol monobutyl ether, heat to 70-80°C and stir until melted, add polyamino NP-Si flame retardant and propylene glycol methyl ether, heat to 90-100°C and keep warm for 1-2h, cool to 80-90°C, add emulsifier, keep warm for 30-40min, cool to 75-85°C, add deionized water, keep warm for 1-2h, discharge and obtain composite water-based epoxy emulsion.

[0015] Further, the preparation of the composite halloysite nanotube hybrid comprises the following steps:

[0016] (1) mixing halloysite nanotubes, hexadecyltrimethylammonium bromide, ammonium molybdate tetrahydrate, thiourea and deionized water, performing ultrasonic dispersion for 10-15 minutes, transferring the mixture to a reaction kettle, maintaining the mixture at 168-172° C. for 9-10 hours, cooling, centrifuging, washing and drying to obtain a halloysite nanotube hybrid;

[0017] (2) Mixing Tris-HCl buffer and anhydrous ethanol, adding halloysite nanotube hybrid, ultrasonically stirring for 30-40 minutes, adding dopamine hydrochloride, keeping warm at 58-62°C for 10-12 hours, adding 3-(2,3-epoxypropoxy)propyltrimethoxysilane, keeping warm at 58-62°C for 10-12 hours, washing, filtering, and drying to obtain modified halloysite nanotube hybrid;

[0018] (3) Under a nitrogen atmosphere, the modified halloysite nanotube hybrid, the polyamino-containing NP-Si flame retardant, and ethanol are mixed and kept at 35-45° C. for 1-2 hours to obtain a composite halloysite nanotube hybrid.

[0019] Furthermore, the mass ratio of epoxy resin E51, epoxy resin E20, dipropylene glycol methyl ether, ethylene glycol monobutyl ether, polyamino-containing NP-Si flame retardant, propylene glycol methyl ether, and emulsifier is 36:24:3:2:6.4:2:7.8.

[0020] Furthermore, the mass ratio of the modified halloysite nanotube hybrid and the polyamino-containing NP-Si flame retardant is 3:4.

[0021] Further, the preparation of the polyamino-containing NP-Si flame retardant comprises the following steps:

[0022] A. Mix deionized water, propanol, acetonitrile and tetraethylammonium hydroxide, add γ-aminopropyltriethoxysilane, stir for 8-12 minutes, heat to 58-62°C and keep warm for 22-24 hours, cool, place in tetrahydrofuran at 0°C, transfer to 0°C until precipitation is generated, filter, repeatedly place in tetrahydrofuran at 0°C for precipitation 3-5 times, and dry to obtain polyamino POSS;

[0023] B. Mix 1,5-diaminonaphthalene, polyamino POSS and ethanol, add a mixture of terephthalaldehyde and ethanol, heat to 58-62°C and keep warm for 5-6 hours, add a mixture of DOPO and ethanol, heat to 78-82°C and keep warm for 6-7 hours, cool, filter, wash, dry and grind to obtain a polyamino NP-Si flame retardant.

[0024] Beneficial effects of the present invention:

[0025] The present invention provides a fireproof heat-insulating coating material and a preparation process thereof. By adjusting the composition and process, the prepared heat-insulating coating material has the characteristics of being non-toxic and harmless and easy to construct. At the same time, it has high fire retardancy and water resistance and is friendly to the human body and the environment.

[0026] In order to improve the fireproof and heat-insulating properties of coating materials, halloysite nanotubes and molybdenum disulfide with low thermal conductivity and good chemical stability are introduced into the coating materials as fireproof fillers, and molybdenum disulfide is in situ grown on the surface of halloysite nanotubes to prepare halloysite nanotube hybrids. Multi-size hybridization is used to construct a complex flame retardant and fireproof network. In order to improve the uniformity of the dispersion of halloysite nanotube hybrids in coating materials, the halloysite nanotube hybrids are modified. Dopamine and silane coupling agent 3-(2,3-epoxypropoxy)propyltrimethoxysilane are used as modifiers. 3-(2,3-epoxypropoxy)propyltrimethoxysilane is used to graft dopamine, and the halloysite nanotube hybrid is double-layer modified to obtain epoxidized halloysite nanotube hybrids. Then, the epoxy-amino reaction is used to graft polyamino-containing NP-Si flame retardants, thereby greatly improving the flame retardancy and smoke suppression of the halloysite nanotube hybrids and improving the safety and fireproof properties of the coating materials.

[0027] The polyamino-containing NP-Si flame retardant is synthesized using polyamino POSS, terephthalaldehyde, 1,5-diaminonaphthalene and DOPO as raw materials. The rich amino groups in the polyamino-containing NP-Si flame retardant can participate in the curing reaction of the coating material, improve the interface compatibility between the flame retardant filler and the coating material matrix, the introduced POSS improves the water resistance of the coating material, the introduced naphthalene ring structure improves the thermal performance of the coating material, and the PN-Si element achieves a synergistic flame retardant effect, giving the composite material high flame retardancy.

[0028] In order to solve the problems of poor water resistance and stability and high VOC of coating materials currently faced by the market, the present invention uses citraconic anhydride, itaconic anhydride and polyethylene glycol as raw materials, prepares an environmentally friendly epoxy emulsifier without adding a catalyst, then introduces a polyethylene glycol segment containing a hydrophilic ethylene oxide segment by reacting with an epoxy group, introduces an NP-Si flame retardant element by reacting an amino group of a polyamino-containing NP-Si flame retardant with an epoxy group, and obtains a composite water-based epoxy emulsion with high flame retardancy and good adhesion to a substrate under the action of the environmentally friendly epoxy emulsifier, and uses the composite water-based epoxy emulsion as a base material for coating materials, thereby greatly improving the water resistance and flame retardancy of the coating. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0031] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0032] Embodiment 1: A process for preparing a fireproof and heat-insulating coating material, comprising the following steps:

[0033] S1: adding titanium dioxide, fumed silica, and composite halloysite nanotube hybrid into a stirring tank, stirring and grinding to obtain a slurry;

[0034] S2: mixing the composite water-based epoxy emulsion, the additive and the slurry, adding the curing agent, stirring and discharging the material to obtain a fireproof and heat-insulating coating material;

[0035] The auxiliary agent is a wetting agent, a dispersant, and a defoaming agent mixed in a mass ratio of 2:1:1; the curing agent is an amine curing agent;

[0036] The raw material composition of the fireproof and heat-insulating coating material is as follows, by weight: 55 parts of composite waterborne epoxy emulsion, 1 part of auxiliary agent, 5 parts of curing agent, 1 part of titanium dioxide, 2 parts of fumed silica, and 6 parts of composite halloysite nanotube hybrid;

[0037] The preparation of the composite waterborne epoxy emulsion comprises the following steps:

[0038] 1) Mix 0.56 g of citraconic anhydride, 0.56 g of itaconic anhydride and 20 g of polyethylene glycol, heat to 78°C and keep warm for 2 h, add 1.2 g of epoxy resin E51 and 0.8 g of epoxy resin E20, heat to 118°C and keep warm for 4 h, cool to obtain an emulsifier;

[0039] 2) 36g of epoxy resin E51, 24g of epoxy resin E20, 5g of dipropylene glycol methyl ether, and 2g of ethylene glycol monobutyl ether were mixed, heated to 70°C and stirred until melted, 6.4g of polyamino NP-Si flame retardant and 2g of propylene glycol methyl ether were added, the temperature was raised to 90°C and kept for 2h, the temperature was lowered to 80°C, 7.8g of emulsifier was added, and the temperature was kept for 30min, the temperature was lowered to 75°C, deionized water was added, and the temperature was kept for 1h, and the material was discharged to obtain a composite water-based epoxy emulsion with a solid content of 30%;

[0040] The preparation of the composite halloysite nanotube hybrid comprises the following steps:

[0041] 1) 1.2 g of halloysite nanotubes, 0.4 g of hexadecyltrimethylammonium bromide, 0.8 g of ammonium molybdate tetrahydrate, 0.8 g of thiourea, and 200 mL of deionized water were mixed, ultrasonically dispersed for 10 min, transferred to a reactor, kept at 168 ° C for 10 h, cooled, centrifuged, washed, and dried to obtain a halloysite nanotube hybrid;

[0042] 2) Mix 250 mL of Tris-HCl buffer with a pH of 8.5 and 50 mL of anhydrous ethanol, add 2 g of halloysite nanotube hybrid, stir ultrasonically for 30 min, add 0.8 g of dopamine hydrochloride, keep warm at 58 ° C for 12 h, add 8 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, keep warm at 58 ° C for 12 h, wash, filter, and dry to obtain a modified halloysite nanotube hybrid;

[0043] 3) Under nitrogen atmosphere, 3 g of modified halloysite nanotube hybrid, 4 g of polyamino-containing NP-Si flame retardant, and 30 mL of ethanol were mixed and kept at 35° C. for 2 h to obtain a composite halloysite nanotube hybrid;

[0044] The preparation of the polyamino-containing NP-Si flame retardant comprises the following steps:

[0045] A. Mix 4.5 mL of deionized water, 2 mL of propanol, 0.5 mL of acetonitrile, and 0.1 mL of tetraethylammonium hydroxide, add 11 g of γ-aminopropyltriethoxysilane, stir for 8 min, heat to 58 ° C and keep warm for 24 h, cool, place in tetrahydrofuran at 0 ° C, transfer to 0 ° C until precipitation is generated, filter, repeatedly place in tetrahydrofuran at 0 ° C for precipitation 3 times, and dry to obtain polyamino POSS;

[0046] B. Mix 5.3 g 1,5-diaminonaphthalene, 28.1 g polyamino POSS, and 50 mL ethanol, add a mixed solution of 13.4 g terephthalaldehyde and 50 mL ethanol, heat to 58°C and keep warm for 6 hours, add a mixed solution of 25 g DOPO and 100 mL ethanol, heat to 78°C and keep warm for 7 hours, cool, filter, wash, dry, and grind to obtain a polyamino NP-Si flame retardant.

[0047] Embodiment 2: A process for preparing a fireproof and heat-insulating coating material, comprising the following steps:

[0048] S1: adding titanium dioxide, fumed silica, and composite halloysite nanotube hybrid into a stirring tank, stirring and grinding to obtain a slurry;

[0049] S2: mixing the composite water-based epoxy emulsion, the additive and the slurry, adding the curing agent, stirring and discharging the material to obtain a fireproof and heat-insulating coating material;

[0050] The auxiliary agent is a wetting agent, a dispersant, and a defoaming agent mixed in a mass ratio of 2:1:1; the curing agent is an amine curing agent;

[0051] The raw material composition of the fireproof and heat-insulating coating material is as follows, by weight: 63 parts of composite waterborne epoxy emulsion, 2 parts of auxiliary agent, 8 parts of curing agent, 3 parts of titanium dioxide, 3 parts of fumed silica, and 8 parts of composite halloysite nanotube hybrid;

[0052] The preparation of the composite waterborne epoxy emulsion comprises the following steps:

[0053] 1) 0.56 g of citraconic anhydride, 0.56 g of itaconic anhydride and 20 g of polyethylene glycol were mixed, heated to 80°C and kept warm for 1.5 h, 1.2 g of epoxy resin E51 and 0.8 g of epoxy resin E20 were added, the temperature was raised to 120°C and kept warm for 3.5 h, and then cooled to obtain an emulsifier;

[0054] 2) 36g of epoxy resin E51, 24g of epoxy resin E20, 5g of dipropylene glycol methyl ether and 2g of ethylene glycol monobutyl ether were mixed, heated to 75°C and stirred until melted, 6.4g of polyamino NP-Si flame retardant and 2g of propylene glycol methyl ether were added, the temperature was raised to 95°C and kept for 1.5h, the temperature was lowered to 85°C, 7.8g of emulsifier was added, and the temperature was kept for 35min, the temperature was lowered to 80°C, deionized water was added, and the temperature was kept for 1.5h, and the material was discharged to obtain a composite waterborne epoxy emulsion with a solid content of 30%;

[0055] The preparation of the composite halloysite nanotube hybrid comprises the following steps:

[0056] 1) 1.2 g of halloysite nanotubes, 0.4 g of hexadecyltrimethylammonium bromide, 0.8 g of ammonium molybdate tetrahydrate, 0.8 g of thiourea, and 200 mL of deionized water were mixed, ultrasonically dispersed for 12 min, transferred to a reactor, kept at 170 ° C for 9.5 h, cooled, centrifuged, washed, and dried to obtain a halloysite nanotube hybrid;

[0057] 2) Mix 250 mL of Tris-HCl buffer with a pH of 8.5 and 50 mL of anhydrous ethanol, add 2 g of halloysite nanotube hybrid, stir ultrasonically for 35 min, add 0.8 g of dopamine hydrochloride, keep warm at 60°C for 11 h, add 8 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, keep warm at 60°C for 11 h, wash, filter, and dry to obtain a modified halloysite nanotube hybrid;

[0058] 3) Under nitrogen atmosphere, 3 g of modified halloysite nanotube hybrid, 4 g of polyamino-containing NP-Si flame retardant, and 30 mL of ethanol were mixed and kept at 40° C. for 1.5 h to obtain a composite halloysite nanotube hybrid;

[0059] The preparation of the polyamino-containing NP-Si flame retardant comprises the following steps:

[0060] A. Mix 4.5 mL of deionized water, 2 mL of propanol, 0.5 mL of acetonitrile, and 0.1 mL of tetraethylammonium hydroxide, add 11 g of γ-aminopropyltriethoxysilane, stir for 10 min, heat to 60 ° C and keep warm for 23 h, cool, place in tetrahydrofuran at 0 ° C, transfer to 0 ° C until precipitation is generated, filter, repeatedly place in tetrahydrofuran at 0 ° C for 4 times, and dry to obtain polyamino POSS;

[0061] B. Mix 5.3 g 1,5-diaminonaphthalene, 28.1 g polyamino POSS, and 50 mL ethanol, add a mixed solution of 13.4 g terephthalaldehyde and 50 mL ethanol, heat to 60°C and keep warm for 5.5 h, add a mixed solution of 25 g DOPO and 100 mL ethanol, heat to 80°C and keep warm for 6.5 h, cool, filter, wash, dry, and grind to obtain a polyamino NP-Si flame retardant.

[0062] Embodiment 3: A process for preparing a fireproof and heat-insulating coating material, comprising the following steps:

[0063] S1: adding titanium dioxide, fumed silica, and composite halloysite nanotube hybrid into a stirring tank, stirring and grinding to obtain a slurry;

[0064] S2: mixing the composite water-based epoxy emulsion, the additive and the slurry, adding the curing agent, stirring and discharging the material to obtain a fireproof and heat-insulating coating material;

[0065] The auxiliary agent is a wetting agent, a dispersant, and a defoaming agent mixed in a mass ratio of 2:1:1; the curing agent is an amine curing agent;

[0066] The raw material composition of the fireproof and heat-insulating coating material is as follows, by weight: 70 parts of composite waterborne epoxy emulsion, 4 parts of auxiliary agent, 12 parts of curing agent, 5 parts of titanium dioxide, 4 parts of fumed silica, and 12 parts of composite halloysite nanotube hybrid;

[0067] The preparation of the composite waterborne epoxy emulsion comprises the following steps:

[0068] 1) Mix 0.56 g of citraconic anhydride, 0.56 g of itaconic anhydride and 20 g of polyethylene glycol, heat to 82°C and keep warm for 1 hour, add 1.2 g of epoxy resin E51 and 0.8 g of epoxy resin E20, heat to 122°C and keep warm for 3 hours, cool to obtain an emulsifier;

[0069] 2) 36g of epoxy resin E51, 24g of epoxy resin E20, 5g of dipropylene glycol methyl ether and 2g of ethylene glycol monobutyl ether were mixed, heated to 80°C and stirred until melted, 6.4g of polyamino NP-Si flame retardant and 2g of propylene glycol methyl ether were added, the temperature was raised to 100°C and kept for 1h, the temperature was lowered to 90°C, 7.8g of emulsifier was added, and the temperature was kept for 40min, the temperature was lowered to 85°C, deionized water was added, and the temperature was kept for 2h, and the material was discharged to obtain a composite waterborne epoxy emulsion with a solid content of 30%;

[0070] The preparation of the composite halloysite nanotube hybrid comprises the following steps:

[0071] 1) 1.2 g of halloysite nanotubes, 0.4 g of hexadecyltrimethylammonium bromide, 0.8 g of ammonium molybdate tetrahydrate, 0.8 g of thiourea, and 200 mL of deionized water were mixed, ultrasonically dispersed for 15 min, transferred to a reactor, kept at 172 ° C for 9 h, cooled, centrifuged, washed, and dried to obtain a halloysite nanotube hybrid;

[0072] 2) Mix 250 mL of Tris-HCl buffer with a pH of 8.5 and 50 mL of anhydrous ethanol, add 2 g of halloysite nanotube hybrid, stir ultrasonically for 40 min, add 0.8 g of dopamine hydrochloride, keep warm at 62 ° C for 10 h, add 8 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, keep warm at 62 ° C for 10 h, wash, filter, and dry to obtain a modified halloysite nanotube hybrid;

[0073] 3) Under nitrogen atmosphere, 3 g of modified halloysite nanotube hybrid, 4 g of polyamino-containing NP-Si flame retardant, and 30 mL of ethanol were mixed and kept at 45° C. for 1 h to obtain a composite halloysite nanotube hybrid;

[0074] The preparation of the polyamino-containing NP-Si flame retardant comprises the following steps:

[0075] A. Mix 4.5 mL of deionized water, 2 mL of propanol, 0.5 mL of acetonitrile, and 0.1 mL of tetraethylammonium hydroxide, add 11 g of γ-aminopropyltriethoxysilane, stir for 12 min, heat to 62 ° C and keep warm for 22 h, cool, place in tetrahydrofuran at 0 ° C, transfer to 0 ° C until precipitation is generated, filter, repeatedly place in tetrahydrofuran at 0 ° C for 5 times, and dry to obtain polyamino POSS;

[0076] B. Mix 5.3 g of 1,5-diaminonaphthalene, 28.1 g of polyamino POSS, and 50 mL of ethanol, add a mixed solution of 13.4 g of terephthalaldehyde and 50 mL of ethanol, heat to 62°C and keep warm for 5 hours, add a mixed solution of 25 g of DOPO and 100 mL of ethanol, heat to 82°C and keep warm for 6 hours, cool, filter, wash, dry, and grind to obtain a polyamino NP-Si flame retardant.

[0077] Comparative Example 1: Taking Example 3 as the control group, the modified halloysite nanotube hybrid was replaced by halloysite nanotubes, and the other processes were normal.

[0078] Comparative Example 2: Taking Example 3 as the control group, the composite water-based epoxy emulsion was replaced with water-based epoxy emulsion (99%, Hubei Chengfeng Chemical Co., Ltd.), and the other processes were normal.

[0079] Comparative Example 3: Example 3 was used as the control group, in which no polyamino-containing NP-Si flame retardant was prepared, and other processes were normal.

[0080] Source of raw materials (for demonstration only):

[0081] Titanium dioxide QF0122: Hubei Qifei Pharmaceutical Chemical Co., Ltd.; fumed silica S26899: Shanghai Yuanye Biotechnology Co., Ltd.; wetting agent T-70: Hanke Chemical; dispersant CP88: Linyi Guoli Chemical Co., Ltd.; defoamer (industrial grade): Jiangsu Duoyang Bioengineering Technology Co., Ltd.; epoxy resin E51 (99%): Hubei Chengfeng Chemical Co., Ltd.; epoxy resin E20: Baling Petrochemical; ethylene glycol monobutyl ether 20240512: Shandong Jinshengrun Chemical Co., Ltd.; amine curing agent (tetraethylene pentamine) T103795, citraconic anhydride C106959, itaconic anhydride I132081, polyethylene glycol P103719, dipropylene glycol methyl ether D108833, propylene glycol methyl ether M105264, halloysite Nanotubes H431905, hexadecyltrimethylammonium bromide H108983, ammonium molybdate tetrahydrate A597691, thiourea T112512, Tris-HCl buffer T301503, dopamine hydrochloride D408026, 3-(2,3-epoxypropoxy)propyltrimethoxysilane G134407, tetraethylammonium hydroxide T102754, γ-aminopropyltriethoxysilane A107147, tetrahydrofuran T431413, 1,5-diaminonaphthalene D135799, terephthalaldehyde P105980, DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) D102416: Aladdin reagent; anhydrous ethanol, propanol, acetonitrile, analytical grade: Sinopharm reagent.

[0082] Performance test: The coating materials prepared in the embodiments and comparative examples were tested for performance:

[0083] Thermal conductivity: Apply the coating material to the hydrophobic silicone rubber surface 5mm by brushing, cure, dry and remove, cut into 20mm×15mm×5mm coating pieces, and measure the thermal conductivity using a thermal constant analyzer at 26℃;

[0084] Flame retardancy: The coating material is applied by brushing on the hydrophobic silicone rubber surface 5mm, cured, dried and removed, cut into 20mm×15mm×5mm coating pieces, and subjected to UL-94 vertical combustion rating test;

[0085] Adhesion: Test adhesion according to GB / T9286-2021, use the 100-grid method, and use a magnifying glass to observe the peeling of the paint film in the grid area. Rating standard: Level 0-the cutting edge is completely smooth and there is no peeling; Level 1-there is a little paint film peeling at the intersection of the cuts, but the affected area is not significantly greater than 5%; Level 2-the affected cross-cut area is 5-15%; Level 3-the affected cross-cut area is 15-35%; Level 4-the affected cross-cut area is 35-65%;

[0086] Water resistance: The coating material was coated on a 145mm×95mm×0.2mm glass sheet, immersed in 5% NaCl for 240h at 25°C, taken out and wiped dry, and the surface was observed for blistering, breakage, etc. If there was no blistering, it was qualified, otherwise it was unqualified; the results are shown in Table 1 below;

[0087] Table 1

[0088]

[0089] The present invention provides a fireproof heat-insulating coating material and a preparation process thereof. By adjusting the composition and process, the prepared heat-insulating coating material has the characteristics of being non-toxic and harmless and easy to construct. At the same time, it has high flame retardancy and water resistance and is friendly to the human body and the environment.

[0090] Example 3 is compared with Comparative Example 1 and Comparative Example 3. In order to improve the fireproof and heat-insulating properties of the coating material, halloysite nanotubes and molybdenum disulfide with lower thermal conductivity and better chemical stability are introduced into the coating material as fireproof fillers, molybdenum disulfide is in situ grown on the surface of the halloysite nanotubes to prepare halloysite nanotube hybrids, and a complex flame-retardant and fireproof network is constructed by multi-size hybridization. In order to improve the uniformity of the dispersion of the halloysite nanotube hybrid in the coating material, the halloysite nanotube hybrid is modified, dopamine and silane coupling agent 3-(2,3-epoxypropoxy)propyltrimethoxysilane are used as modifiers, dopamine is grafted onto the end of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, and the halloysite nanotube hybrid is double-layered. The invention discloses a novel nanostructured composite material comprising a nanostructured composite material and a nanostructured composite material. The nanostructured composite material is modified to obtain an epoxidized halloysite nanotube hybrid; and then the epoxy-amino reaction is used to graft a polyamino-containing NP-Si flame retardant, thereby greatly improving the flame retardancy and smoke suppression of the halloysite nanotube hybrid and improving the safety and fire resistance of the coating material; wherein the polyamino-containing NP-Si flame retardant is synthesized using polyamino POSS, terephthalaldehyde, 1,5-diaminonaphthalene and DOPO as raw materials, and the rich amino groups in the polyamino-containing NP-Si flame retardant can participate in the curing reaction of the coating material, thereby improving the interface compatibility between the flame retardant filler and the coating material matrix, the introduced POSS improves the water resistance of the coating material, the introduced naphthalene ring structure improves the thermal performance of the coating material, and the PN-Si element achieves a synergistic flame retardant effect, thereby giving the composite material high flame retardancy.

[0091] Example 3 is compared with Comparative Examples 2 and 3. In order to solve the problems of poor water resistance and stability and high VOC of coating materials currently faced by the market, the present invention uses citraconic anhydride, itaconic anhydride and polyethylene glycol as raw materials, and prepares an environmentally friendly epoxy emulsifier without adding a catalyst. Then, polyethylene glycol containing a hydrophilic ethylene oxide segment reacts with an epoxy group to introduce a polyethylene oxide segment. The NP-Si flame retardant element is introduced by reacting the amino group of a polyamino-containing NP-Si flame retardant with an epoxy group. Under the action of the environmentally friendly epoxy emulsifier, a composite water-based epoxy emulsion with high flame retardancy and good adhesion to a substrate is obtained. The composite water-based epoxy emulsion is used as a base material for coating materials, thereby greatly improving the water resistance and flame retardancy of the coating.

[0092] The above descriptions are only embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A preparation process of a fireproof and heat-insulating coating material, characterized in that: The following steps are involved: S1: adding titanium dioxide, fumed silica, and composite halloysite nanotube hybrid into a stirring tank, stirring and grinding to obtain a slurry; S2: mixing the composite water-based epoxy emulsion, the additive and the slurry, adding the curing agent, stirring and discharging the material to obtain a fireproof and heat-insulating coating material; The preparation of the composite waterborne epoxy emulsion comprises the following steps: 1) Mix citraconic anhydride, itaconic anhydride and polyethylene glycol, heat to 78-82°C and keep warm for 1-2 hours, add epoxy resin E51 and epoxy resin E20, heat to 118-122°C and keep warm for 3-4 hours, cool and obtain an emulsifier; 2) Mix epoxy resin E51, epoxy resin E20, dipropylene glycol methyl ether and ethylene glycol monobutyl ether, heat to 70-80°C and stir until melted, add polyamino NP-Si flame retardant and propylene glycol methyl ether, heat to 90-100°C and keep warm for 1-2h, cool to 80-90°C, add emulsifier, keep warm for 30-40min, cool to 75-85°C, add deionized water, keep warm for 1-2h, discharge and obtain composite waterborne epoxy emulsion; The preparation of the composite halloysite nanotube hybrid comprises the following steps: (1) mixing halloysite nanotubes, hexadecyltrimethylammonium bromide, ammonium molybdate tetrahydrate, thiourea and deionized water, performing ultrasonic dispersion for 10-15 minutes, transferring the mixture to a reaction kettle, maintaining the mixture at 168-172° C. for 9-10 hours, cooling, centrifuging, washing and drying to obtain a halloysite nanotube hybrid; (2) Mixing Tris-HCl buffer and anhydrous ethanol, adding halloysite nanotube hybrid, ultrasonically stirring for 30-40 minutes, adding dopamine hydrochloride, keeping warm at 58-62°C for 10-12 hours, adding 3-(2,3-epoxypropoxy)propyltrimethoxysilane, keeping warm at 58-62°C for 10-12 hours, washing, filtering, and drying to obtain modified halloysite nanotube hybrid; (3) Under a nitrogen atmosphere, the modified halloysite nanotube hybrid, the polyamino-containing NP-Si flame retardant, and ethanol are mixed and kept at 35-45° C. for 1-2 hours to obtain a composite halloysite nanotube hybrid; The preparation of the polyamino-containing NP-Si flame retardant comprises the following steps: A. Mix deionized water, propanol, acetonitrile and tetraethylammonium hydroxide, add γ-aminopropyltriethoxysilane, stir for 8-12 minutes, heat to 58-62°C and keep warm for 22-24 hours, cool, place in tetrahydrofuran at 0°C, transfer to 0°C until precipitation is generated, filter, repeatedly place in tetrahydrofuran at 0°C for precipitation 3-5 times, and dry to obtain polyamino POSS; B. 1,5-diaminonaphthalene, polyamino POSS and ethanol are mixed, a mixture of terephthalaldehyde and ethanol is added, the temperature is raised to 58-62°C and kept warm for 5-6 hours, a mixture of DOPO and ethanol is added, the temperature is raised to 78-82°C and kept warm for 6-7 hours, cooling, filtering, washing, drying and grinding to obtain a polyamino NP-Si flame retardant; The raw material composition of the fireproof and heat-insulating coating material is as follows: 55-70 parts of composite waterborne epoxy emulsion, 1-4 parts of auxiliary agent, 5-12 parts of curing agent, 1-5 parts of titanium dioxide, 2-4 parts of fumed silica, and 6-12 parts of composite halloysite nanotube hybrid, in parts by mass. In the preparation of the composite waterborne epoxy emulsion, the mass ratio of the epoxy resin E51, epoxy resin E20, dipropylene glycol methyl ether, ethylene glycol monobutyl ether, polyamino-containing NP-Si flame retardant, propylene glycol methyl ether, and emulsifier is 36:24:3:2:6.4:2:7.8; In the preparation of the composite halloysite nanotube hybrid, the mass ratio of the modified halloysite nanotube hybrid to the polyamino-containing NP-Si flame retardant is 3:

4.

2. The preparation process of a fireproof and heat-insulating coating material according to claim 1, characterized in that: The auxiliary agent is a wetting agent, a dispersing agent and a defoaming agent mixed in a mass ratio of 2:1:

1.

3. The preparation process of a fireproof and heat-insulating coating material according to claim 1, characterized in that: The curing agent is an amine curing agent.

4. A fireproof and heat-insulating coating material, characterized in that: Prepared according to any one of the preparation processes of claims 1-3.