Light-emitting diode epitaxial wafer and preparation method thereof, and light-emitting diode
By designing a composite P-type semiconductor layer structure in GaN-based light-emitting diodes and utilizing the heterojunction effect of the BN layer, BAsxN1-x layer and periodic structure, the problems of high work function and poor ohmic contact of the P-type GaN layer are solved. The effect of reducing the operating voltage and improving the luminous efficiency is achieved.
Patent Information
- Application Number
- CN202411162496.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Due to the high work function of the P-type GaN layer and poor metal ohmic contact, existing GaN-based light-emitting diodes have high operating voltage and low luminous efficiency, which is especially obvious in high-power LED chips.
A P-type semiconductor layer structure including a BN layer, a BAsxN1-x layer, a periodic structure of a P-type GaN layer, a BAsyN1-y layer, a P-type BzGa1-zN layer, a P-type BαGa1-αN layer and a P-type InGaN layer is adopted. Electron blocking of BN layer, B The uniform hole injection of the AsxN1-x layer, the periodic structure of the heterojunction and the low bandgap width and high carrier mobility of the P-type InGaN layer and the anti-blocking layer effect of the P-type BαGa1-αN layer increase the number of holes. And the recombination efficiency of electrons, reducing the operating voltage and improving the luminous efficiency.
It effectively reduces the operating voltage of the light-emitting diode and improves the luminous efficiency. By optimizing the structure of the P-type semiconductor layer, the hole injection uniformity and carrier tunneling rate are improved, and the luminous efficiency and ohmic contact quality are enhanced.
Smart Images

Figure CN118676277B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor optoelectronic devices, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and a light emitting diode. Background Art
[0002] GaN-based light-emitting diodes are the most widely used LEDs at present. They generally use a P-type GaN layer as the P-type layer. However, due to the high work function of the P-type GaN layer (about 6.12eV), the general metal has poor ohmic contact with it, resulting in high operating voltage and low luminous efficiency. This problem is more obvious in high-power LED chips. The methods for solving this problem in the prior art include: increasing the doping concentration of the P-type GaN layer to increase the hole concentration and improve the ohmic contact. However, too high a doping concentration will reduce the lattice quality of the P-type GaN layer, enhance light absorption, and reduce the luminous efficiency of the LED. Another method is to introduce a transparent conductive layer (ITO, IZO, etc.) between the metal electrode and the P-type GaN layer as a connection. However, these layers will absorb more light and reduce the luminous efficiency. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a light emitting diode epitaxial wafer and a preparation method thereof, which can improve the light emitting efficiency of the light emitting diode and reduce its operating voltage.
[0004] In order to solve the above problems, the present invention discloses a light emitting diode epitaxial wafer, which comprises a substrate, a buffer layer, an N-type semiconductor layer, a multi-quantum well layer and a P-type semiconductor layer sequentially stacked on the substrate; the P-type semiconductor layer comprises a first composite layer, a second composite layer and a third composite layer sequentially stacked on the multi-quantum well layer;
[0005] The first composite layer includes a BN layer and a BAs layer sequentially stacked on the multi-quantum well layer. x N 1-x layer;
[0006] The second composite layer is a periodic structure with a period number of 2 to 10, and each period includes a P-type GaN layer, a BAs y N 1-y Layer and P-type B z Ga 1-z N layers;
[0007] The third composite layer includes a P-type B sequentially stacked on the second composite layer α Ga 1-α N-layer and P-type InGaN layer;
[0008] Among them, x>y, z>α.
[0009] As an improvement of the above technical solution, the thickness of the BN layer is 10nm~20nm; and / or
[0010] The BAs x N 1-x The thickness of the layer is 10nm~20nm, and the value of x ranges from 0.55 to 0.75.
[0011] As an improvement of the above technical solution, the thickness of the P-type GaN layer is 2nm~5nm, and its doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 ; and / or
[0012] The BAs y N 1-y The thickness of the layer is 2nm~5nm, and the value of y ranges from 0.5 to 0.65; and / or
[0013] The P-type B z Ga 1-z The thickness of the N layer is 3nm~8nm, and its doping concentration is 1×10 20 cm -3 ~1×10 22 cm -3 , the value range of z is 0.1~0.3.
[0014] As an improvement of the above technical solution, the P-type B α Ga 1-α The thickness of the N layer is 10nm~30nm, and its doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 , the value range of α is 0.05~0.1; and / or
[0015] The thickness of the P-type InGaN layer is 5nm~20nm, and its doping concentration is 1×10 20 cm -3 ~1×10 22 cm -3 , the In component accounts for 0.1~0.2.
[0016] As an improvement of the above technical solution, z≤0.2, y≤0.62, so that the BAs y N 1-y The lattice constant of the layer is smaller than that of the P-type B z Ga 1-z Lattice constant of the N layer.
[0017] As an improvement of the above technical solution, the P-type Bz Ga 1-z The doping concentration of the N layer is greater than the doping concentration of the P-type GaN layer.
[0018] As an improvement of the above technical solution, the buffer layer is an AlN layer with a thickness of 30nm to 80nm; and / or
[0019] The N-type semiconductor layer is an N-type GaN layer, and its thickness is 1 μm to 5 μm; and / or
[0020] The multi-quantum well layer is a periodic structure formed by alternately stacking InGaN quantum well layers and GaN quantum barrier layers, the number of periods is 3 to 15, the thickness of the InGaN quantum well layer is 3nm to 5nm, and the thickness of the GaN quantum barrier layer is 8nm to 15nm.
[0021] Correspondingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned light-emitting diode epitaxial wafer, and comprises:
[0022] Providing a substrate, and sequentially growing a buffer layer, an N-type semiconductor layer, a multi-quantum well layer, and a P-type semiconductor layer on the substrate; the P-type semiconductor layer comprises a first composite layer, a second composite layer, and a third composite layer sequentially stacked on the multi-quantum well layer;
[0023] The first composite layer includes a BN layer and a BAs layer sequentially stacked on the multi-quantum well layer. x N 1-x layer;
[0024] The second composite layer is a periodic structure with a period number of 2 to 10, and each period includes a P-type GaN layer, a BAs y N 1-y Layer and P-type B z Ga 1-z N layers;
[0025] The third composite layer includes a P-type B sequentially stacked on the second composite layer α Ga 1-α N-layer and P-type InGaN layer;
[0026] Among them, x>y, z>α.
[0027] As an improvement of the above technical solution, the growth temperature of the BN layer is 1200° C. to 1300° C., and the growth pressure is 50 torr to 200 torr; and / or
[0028] The BAs x N 1-xThe growth temperature of the layer is 850°C to 1000°C and the growth pressure is 100 torr to 300 torr; and / or
[0029] The growth temperature of the P-type GaN layer is 900° C. to 1100° C., and the growth pressure is 100 torr to 300 torr; and / or
[0030] The BAs y N 1-y The growth temperature of the layer is 850°C to 1000°C and the growth pressure is 100 torr to 300 torr; and / or
[0031] The P-type B z Ga 1-z The growth temperature of the N layer is 1000℃~1200℃, and the growth pressure is 100torr~500torr;
[0032] The P-type B α Ga 1-α The growth temperature of the N layer is 1000°C to 1200°C, and the growth pressure is 100 torr to 500 torr; and / or
[0033] The growth temperature of the P-type InGaN layer is 800° C. to 900° C., and the growth pressure is 100 torr to 500 torr.
[0034] Correspondingly, the present invention also discloses a light emitting diode, which includes the light emitting diode epitaxial wafer mentioned above.
[0035] The implementation of the present invention has the following beneficial effects:
[0036] In the light emitting diode epitaxial wafer of the present invention, the first composite layer, the second composite layer and the third composite layer sequentially stacked on the multi-quantum well layer are used as the P-type semiconductor layer. The first composite layer includes a BN layer and a BAs x N 1-x layer; the BN layer can enhance the blocking effect on electrons and cooperate with BAs x N 1-x The second composite layer is a periodic structure with a period number of 2 to 10. Each period includes a sequentially stacked P-type GaN layer, BAs y N 1-y Layer and P-type B z Ga 1-z N layer; wherein, through periodic stacking, the P-type GaN layer and the P-type B z Ga 1-z The N layer forms a heterojunction structure, which can accelerate holes, while BAs with low bandgap width and high carrier mobilityy N 1-y The third composite layer includes a P-type B layer stacked on the second composite layer. α Ga 1-α N layer and P-type InGaN layer; the work function of the P-type InGaN layer is small, which helps to form a good ohmic contact with the metal electrode later, while the P-type B α Ga 1-α The N layer can narrow the barrier region of the anti-blocking layer generated between the electrode metal and the P-type semiconductor layer, increase the probability of carrier tunneling through the metal and semiconductor contact, reduce the operating voltage, and improve the luminous efficiency. In summary, the P-type semiconductor layer of the present invention effectively reduces the operating voltage of the light-emitting diode and improves the luminous efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a schematic structural diagram of a light emitting diode epitaxial wafer in one embodiment of the present invention;
[0038] Figure 2 It is a flow chart of a method for preparing a light emitting diode epitaxial wafer in one embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0040] refer to Figure 1 The present invention discloses a light emitting diode epitaxial wafer, which includes a substrate 100, a buffer layer 200, an N-type semiconductor layer 300, a multi-quantum well layer 400 and a P-type semiconductor layer 500, which are sequentially stacked on the substrate 100. The P-type semiconductor layer 500 includes a first composite layer 510, a second composite layer 520 and a third composite layer 530, which are sequentially stacked on the multi-quantum well layer 400. The first composite layer 510 includes a BN layer 511 and a BAs x N 1-x The second composite layer 520 is a periodic structure, each period includes a P-type GaN layer 521, a BAs y N 1-y Layer 522 and P-type B z Ga 1-z The third composite layer 530 includes a P-type B layer sequentially stacked on the second composite layer 520. α Ga 1-αN layer 531 and P-type InGaN layer 532. Based on the above-mentioned P-type semiconductor layer 500, on the one hand, the BN layer 511 can effectively block the electrons overflowing from the multi-quantum well layer 400 from entering the P-type semiconductor layer 500, and non-radiative recombination occurs; at the same time, the BN layer 511 can also block holes and cooperate with the BAs with high carrier mobility. x N 1-x Layer 512 allows holes to be more uniformly injected into the multi-quantum well layer 400, thereby improving the luminous efficiency. y N 1-y Layer 522 has the advantages of low bandgap width and high carrier mobility, which greatly improves the mobility of holes, helps to improve the recombination efficiency of holes and electrons, improves luminous efficiency, reduces operating voltage, and helps to reduce ohmic contact resistance. P-type GaN layer 521 and P-type B z Ga 1-z The N layer 523 is the main source of holes, and forms a heterojunction through periodic cycles, which accelerates holes and further improves the recombination efficiency of holes and electrons. α Ga 1-α The N layer 531 and the P-type InGaN layer 532 are the surface layers. The P-type InGaN layer 532 has a lower work function, which is helpful to form a good ohmic contact with the metal electrode later. α Ga 1-α The N layer 531 can narrow the barrier region of the anti-blocking layer generated between the metal and the P-type semiconductor layer, increase the probability of carrier tunneling through the contact between the metal and the semiconductor, reduce the operating voltage, and improve the luminous efficiency.
[0041] The thickness of the BN layer 511 is 10 nm to 30 nm. If the thickness is too large, the efficiency of hole injection into the multi-quantum well layer 400 is affected. Exemplarily, the thickness of the BN layer 511 is 12 nm, 16 nm, 20 nm or 25 nm, but not limited thereto. Preferably, the thickness of the BN layer 511 is 10 nm to 20 nm.
[0042] Among them, BAs x N 1-x The value range of x in layer 512 is 0.46~0.8. If x<0.46, then BAs x N 1-x The band gap width of layer 512 is large, and the carrier mobility is low, which makes it difficult to effectively improve the luminous efficiency. If x>0.8, then BAs x N 1-x The growth difficulty of layer 512 is relatively high. Preferably, the value range of x is 0.55-0.75, and exemplarily is 0.58, 0.62, 0.65, 0.71 or 0.74, but not limited thereto.
[0043] BAs x N 1-x The thickness of the layer 512 is 10 nm to 30 nm, exemplarily 14 nm, 18 nm, 22 nm or 26 nm, but not limited thereto, preferably 10 nm to 20 nm.
[0044] The number of periods of the second composite layer 520 is 2-10, exemplarily 3, 5, 7 or 9, but not limited thereto, and preferably 3-6.
[0045] The doping element of the P-type GaN layer 521 is Mg, but not limited thereto. The doping concentration of the P-type GaN layer 521 is 5×10 18 cm -3 ~1×10 21 cm -3 ; An exemplary value is 7×10 18 cm -3 , 2×10 19 cm -3 , 6×10 19 cm -3 , 3×10 20 cm -3 or 9×10 20 cm -3 , but not limited thereto. Preferably 1×10 19 cm -3 ~1×10 21 cm -3 .
[0046] The thickness of the P-type GaN layer 521 is 1 nm to 5 nm, exemplarily 1 nm, 2 nm, 3 nm or 4 nm, but not limited thereto, preferably 2 nm to 5 nm.
[0047] Among them, BAs y N 1-y The value range of y in layer 522 is 0.46~0.8. If y<0.46, then BAs y N 1-y The band gap width of layer 522 is large, and the carrier mobility is low, which makes it difficult to effectively improve the luminous efficiency. If y>0.8, then BAs y N 1-y The growth of layer 522 is difficult. In addition, in the present invention, y<x is controlled to optimize the distribution and mobility of holes. Preferably, the value range of y is 0.5 to 0.65. Exemplary values are 0.53, 0.55, 0.58, 0.62 or 0.64, but not limited thereto.
[0048] BAs y N 1-yThe thickness of the layer 522 is 1 nm to 5 nm, exemplarily 1.5 nm, 2 nm, 3 nm, 3.5 nm or 4 nm, but not limited thereto, preferably 2 nm to 5 nm.
[0049] Among them, P type B z Ga 1-z The doping element of the N layer 523 is Mg, but is not limited thereto. z Ga 1-z The doping concentration of the N layer 523 is 5×10 19 cm -3 ~1×10 22 cm -3 , exemplarily 8×10 19 cm -3 , 2×10 20 cm -3 , 8×10 20 cm -3 , 3×10 21 cm -3 or 7×10 21 cm -3 , but not limited thereto. Preferably 1×10 20 cm -3 ~1×10 22 cm -3 , more preferably 1×10 20 cm -3 ~1×10 21 cm -3 Since B atoms are small in size, they can be inserted into or fill the surface vacant positions caused by dislocations to reduce defects. Therefore, the crystal quality of this layer is higher, so a higher doping concentration is used.
[0050] P-type B z Ga 1-z The value range of z in the N layer 523 is 0.1-0.4, exemplarily 0.12, 0.17, 0.24, 0.28, 0.35 or 0.38, but not limited thereto, and preferably 0.1-0.3.
[0051] P-type B z Ga 1-z The thickness of the N layer 523 is 2 nm to 10 nm, exemplarily 3 nm, 5 nm, 7 nm or 9 nm, but not limited thereto, preferably 3 nm to 8 nm.
[0052] Among them, P type B α Ga 1-αThe value range of α in the N layer 531 is 0.05-0.2, and is 0.08, 0.1, 0.13, 0.17 or 0.19, but is not limited thereto. Preferably, it is 0.05-0.1. In addition, in the present invention, z>α is controlled to improve the crystal quality of the P-type semiconductor layer 500.
[0053] P-type B α Ga 1-α The doping element of the N layer 531 is Mg, but is not limited thereto. α Ga 1-α The doping concentration of the N layer 531 is 5×10 18 cm -3 ~1×10 21 cm -3 ; An exemplary value is 7×10 18 cm -3 , 2×10 19 cm -3 , 6×10 19 cm -3 , 3×10 20 cm -3 or 9×10 20 cm -3 , but not limited thereto. Preferably 1×10 19 cm -3 ~1×10 21 cm -3 .
[0054] P-type B α Ga 1-α The thickness of the N layer 531 is 10 nm to 50 nm, and is exemplarily 13 nm, 15 nm, 24 nm, 33 nm, 40 nm or 45 nm, but is not limited thereto, and is preferably 10 nm to 30 nm.
[0055] The ratio of In component in the P-type InGaN layer 532 is 0.05-0.2, exemplarily 0.08, 0.12, 0.14 or 0.16, but not limited thereto, and preferably 0.1-0.2.
[0056] The doping element of the P-type InGaN layer 532 is Mg, but is not limited thereto. The doping concentration of the P-type InGaN layer 532 is 5×10 19 cm -3 ~1×10 22 cm -3 , exemplarily 8×10 19 cm -3 , 2×10 20 cm -3 , 8×10 20 cm -3, 3×10 21 cm -3 or 7×10 21 cm -3 , but not limited thereto. Preferably 1×10 20 cm -3 ~1×10 22 cm -3 .
[0057] The thickness of the P-type InGaN layer 532 is 5 nm to 30 nm, exemplarily 8 nm, 12 nm, 16 nm, 22 nm or 24 nm, but not limited thereto, preferably 5 nm to 20 nm.
[0058] Preferably, in one embodiment of the present invention, z≤0.2 and y≤0.62 are controlled so that BAs y N 1-y The lattice constant of layer 522 is smaller than that of P-type B z Ga 1-z The lattice constant of the N layer 523. Based on this control, the overall lattice quality of the second composite layer 520 can be effectively improved, the operating voltage can be further reduced, and the luminous efficiency can be improved.
[0059] Preferably, in one embodiment of the present invention, P-type B z Ga 1-z The doping concentration of the N layer 523 is greater than the doping concentration of the P-type GaN layer 521. Based on this control, the light emitting efficiency can be further improved.
[0060] The substrate 100 is a sapphire substrate, a silicon substrate or a silicon carbide substrate, but is not limited thereto.
[0061] The buffer layer 200 is an AlN layer or an AlGaN layer, but is not limited thereto. The buffer layer 200 has a thickness of 20 nm to 80 nm.
[0062] The N-type semiconductor layer 300 may be an N-type GaN layer or an N-type AlGaN layer, but is not limited thereto. Preferably, in one embodiment, the N-type semiconductor layer 300 is an N-type GaN layer, and its doping element is Si, but is not limited thereto. The doping concentration is 5×10 18 cm -3 ~5×10 19 cm -3 , thickness is 1μm~5μm.
[0063] The multi-quantum well layer 400 is an InGaN-GaN type multi-quantum well layer or an InGaN-AlGaN type multi-quantum well layer, but is not limited thereto. Preferably, in one embodiment, the multi-quantum well layer 400 is a periodic structure formed by alternating InGaN quantum well layers 410 and GaN quantum barrier layers 420, the number of periods is 3 to 15, the thickness of the InGaN quantum well layer 410 is 3 nm to 5 nm, and the thickness of the GaN quantum barrier layer 420 is 8 nm to 15 nm.
[0064] Preferably, in one embodiment, the light emitting diode epitaxial wafer further includes a non-doped GaN layer 600 , which is disposed between the N-type semiconductor layer 300 and the buffer layer 200 , and has a thickness of 1 μm to 3 μm.
[0065] Preferably, in one embodiment, the light emitting diode epitaxial wafer further includes an electron blocking layer 700, which is an AlGaN layer or an AlInGaN layer, but is not limited thereto, and has a thickness of 10 nm to 40 nm.
[0066] Accordingly, reference Figure 2 The present invention also provides a method for preparing a light emitting diode epitaxial wafer, which is used to prepare the above-mentioned light emitting diode epitaxial wafer, and specifically comprises the following steps:
[0067] S1: providing a substrate;
[0068] S2: sequentially growing a buffer layer, an N-type semiconductor layer, a multi-quantum well layer and a P-type semiconductor layer on the substrate.
[0069] Preferably, in some embodiments of the present invention, step S2 comprises:
[0070] S21: growing a buffer layer on the substrate;
[0071] The buffer layer may be grown by PVD, MOCVD, MBE or VPE, but is not limited thereto.
[0072] Preferably, in one embodiment of the present invention, an AlN layer is grown by PVD as a buffer layer.
[0073] S22: growing a non-doped GaN layer on the buffer layer;
[0074] The non-doped GaN layer may be grown by PVD, MOCVD, MBE or VPE, but is not limited thereto.
[0075] Preferably, in one embodiment of the present invention, the non-doped GaN layer is grown by MOCVD at a growth temperature of 1100° C. to 1150° C. and a growth pressure of 100 torr to 500 torr.
[0076] S23: growing an N-type semiconductor layer on the non-doped GaN layer;
[0077] Here, an N-type GaN layer or an N-type AlGaN layer may be grown by MOCVD, MBE or VPE as the N-type semiconductor layer, but is not limited thereto.
[0078] Preferably, in one embodiment of the present invention, an N-type GaN layer is grown by MOCVD as the N-type semiconductor layer; the growth temperature is 1100° C. to 1150° C., and the growth pressure is 100 torr to 500 torr.
[0079] S24: growing a multi-quantum well layer on the N-type semiconductor layer;
[0080] In one embodiment, the InGaN quantum well layer and the GaN quantum barrier layer may be alternately grown by MOCVD, but is not limited thereto. Specifically, the growth temperature of the InGaN quantum well layer is 740°C to 820°C, and the growth pressure is 100 torr to 300 torr. The growth temperature of the GaN quantum barrier layer is 850°C to 950°C, and the growth pressure is 100 torr to 300 torr.
[0081] S25: growing an electron blocking layer on the multi-quantum well layer;
[0082] In one embodiment, an AlGaN layer is grown by MOCVD as an electron blocking layer, and the growth temperature is 1000° C. to 1200° C. and the growth pressure is 100 torr to 500 torr.
[0083] S26: growing a P-type semiconductor layer on the electron blocking layer;
[0084] Specifically, in one embodiment, step S26 includes the following steps:
[0085] S261: growing a BN layer on the electron blocking layer;
[0086] The BN layer may be grown by PVD or MOCVD, but is not limited thereto.
[0087] Preferably, in one embodiment, the BN layer is grown by MOCVD, and the growth temperature is 1200° C. to 1300° C. and the growth pressure is 50 torr to 200 torr.
[0088] S262: Growth of BAs on BN layer x N 1-x layer, obtaining a first composite layer;
[0089] Among them, BAs can be grown by CVT, PVD or MOCVD x N1-x layer, but not limited to it.
[0090] Preferably, in one embodiment, BAs are grown by MOCVD. x N 1-x layer, the growth temperature is 850℃~1000℃, and the growth pressure is 100torr~300torr.
[0091] S263: growing a second composite layer on the first composite layer;
[0092] In one embodiment, the P-type GaN layer, BAs y N 1-y Layer and P-type B z Ga 1-z N layers, until the second composite layer is obtained;
[0093] Specifically, the growth temperature of the P-type GaN layer is 900°C~1100°C, and the growth pressure is 100torr~300torr; BAs y N 1-y The growth temperature of the layer is 850℃~1000℃, and the growth pressure is 100torr~300torr; P type B z Ga 1-z The growth temperature of the N layer is 1000℃~1200℃, and the growth pressure is 100torr~500torr.
[0094] S264: Growth of P-type B on the second composite layer α Ga 1-α N layers;
[0095] Among them, P-type B can be grown by MOCVD, MBE or VPE α Ga 1-α N layers, but not limited to this.
[0096] Preferably, in one embodiment, P-type B is grown by MOCVD. α Ga 1-α The N layer has a growth temperature of 1000°C~1200°C and a growth pressure of 100torr~500torr.
[0097] S265: In P type B α Ga 1-α A P-type InGaN layer is grown on the N layer;
[0098] The P-type InGaN layer may be grown by MOCVD, MBE or VPE, but is not limited thereto.
[0099] Preferably, in one embodiment, the P-type InGaN layer is grown by MOCVD, and the growth temperature is 800° C. to 900° C. and the growth pressure is 100 torr to 500 torr.
[0100] Correspondingly, the present invention also discloses a light emitting diode, which includes the light emitting diode epitaxial wafer mentioned above.
[0101] The present invention will be further described below with specific embodiments:
[0102] Example 1
[0103] This embodiment provides a light emitting diode epitaxial wafer, which includes a substrate, a buffer layer, a non-doped GaN layer, an N-type semiconductor layer, a multi-quantum well layer, an electron blocking layer and a P-type semiconductor layer stacked in sequence on the substrate.
[0104] The substrate is a sapphire substrate, the buffer layer is an AlN layer with a thickness of 40 nm, the thickness of the undoped GaN layer is 1.5 μm, the N-type semiconductor layer is an N-type GaN layer with a Si doping concentration of 1×10 19 cm -3 , with a thickness of 2μm. The multi-quantum well layer is a periodic structure with 10 periods. Each period includes sequentially stacked InGaN quantum well layers and GaN quantum barrier layers. The thickness of the InGaN quantum well layer is 3.5nm; the thickness of the GaN quantum barrier layer is 10nm. The electron blocking layer is an AlGaN layer with a thickness of 35nm.
[0105] The P-type semiconductor layer includes a first composite layer, a second composite layer and a third composite layer sequentially stacked on the electron blocking layer, and the first composite layer sequentially includes a BN layer and a BAs x N 1-x layer (x = 0.7), the thickness of the BN layer is 18nm; BAs x N 1-x The thickness of the layer is 12nm. The second composite layer is a periodic structure with 5 periods. Each period includes a P-type GaN layer, a BAs y N 1-y Layer (y=0.65) and P-type B z Ga 1-z N layer (z = 0.25); the thickness of the P-type GaN layer is 4nm, and its Mg doping concentration is 1×10 21 cm -3 BAs y N 1-y The thickness of the layer is 3nm; P-type B z Ga 1-z The thickness of the N layer is 6 nm, and its Mg doping concentration is 5×10 20 cm-3 ; The third composite layer includes P type B α Ga 1-α N layer (α=0.08) and P-type InGaN layer; P-type B α Ga 1-α The thickness of the N layer is 20 nm and its Mg doping concentration is 1×10 20 cm -3 ; The In component ratio in the P-type InGaN layer is 0.12, and the Mg doping concentration is 5×10 21 cm -3 , with a thickness of 12nm.
[0106] The method for preparing the light emitting diode epitaxial wafer in this embodiment comprises the following steps:
[0107] (1) Providing a substrate.
[0108] (2) growing a buffer layer on the substrate;
[0109] Among them, an AlN layer is grown by PVD as a buffer layer;
[0110] (3) growing a non-doped GaN layer on the buffer layer;
[0111] The non-doped GaN layer is grown by MOCVD at a growth temperature of 1100° C. and a growth pressure of 200 torr.
[0112] (4) growing an N-type semiconductor layer on the undoped GaN layer;
[0113] The N-type GaN layer is grown by MOCVD as the N-type semiconductor layer, and the growth temperature is 1140° C. and the growth pressure is 200 torr.
[0114] (5) Growing a multi-quantum well layer on the N-type semiconductor layer;
[0115] Specifically, an InGaN quantum well layer and a GaN quantum barrier layer are periodically grown on an N-type semiconductor layer by MOCVD until a multi-quantum well layer is obtained, wherein the growth temperature of the InGaN quantum well layer is 760°C and the growth pressure is 200 torr; the growth temperature of the GaN quantum barrier layer is 890°C and the growth pressure is 200 torr.
[0116] (6) growing an electron blocking layer on the multi-quantum well layer;
[0117] Specifically, the AlGaN layer is grown by MOCVD as an electron blocking layer at a growth temperature of 1050° C. and a growth pressure of 300 torr.
[0118] (7) growing a BN layer on the electron blocking layer;
[0119] Specifically, the BN layer is grown by MOCVD at a growth temperature of 1220° C. and a growth pressure of 100 torr.
[0120] (8) Growth of BAs on BN layer x N 1-x layer, obtaining a first composite layer;
[0121] Specifically, BAs were grown by MOCVD. x N 1-x layer, with a growth temperature of 900°C and a growth pressure of 200 torr.
[0122] (9) growing a second composite layer on the first composite layer;
[0123] Specifically, P-type GaN layers, BAs y N 1-y Layer and P-type B z Ga 1-z N layers, until the second composite layer is obtained;
[0124] Specifically, the growth temperature of the P-type GaN layer is 950°C and the growth pressure is 200 torr; BAs y N 1-y The growth temperature of the layer is 920℃ and the growth pressure is 200torr; P-type B z Ga 1-z The growth temperature of the N layer is 1120°C and the growth pressure is 200 torr.
[0125] (10) Growth of P-type B on the second composite layer α Ga 1-α N layers;
[0126] Specifically, P-type B is grown by MOCVD α Ga 1-α The N layer has a growth temperature of 1100°C and a growth pressure of 200 torr.
[0127] (11) In P type B α Ga 1-α A P-type InGaN layer is grown on the N layer;
[0128] Specifically, the P-type InGaN layer is grown by MOCVD, with a growth temperature of 850° C. and a growth pressure of 200 torr.
[0129] Example 2
[0130] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 1 in that:
[0131] BAsy N 1-y Layer y=0.55; P type B z Ga 1-z In layer N, z=0.12.
[0132] The rest are the same as in Example 1.
[0133] Example 3
[0134] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 2 in that:
[0135] The Mg doping concentration in the P-type GaN layer is 5×10 20 cm -3 ; P-type B z Ga 1-z The Mg doping concentration in the N layer is 3×10 21 cm -3 .
[0136] The rest is the same as Example 2.
[0137] Comparative Example 1
[0138] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:
[0139] The P-type semiconductor layer is a P-type GaN layer with a Mg doping concentration of 5×10 20 cm -3 The thickness is 180nm. The growth temperature of the P-type semiconductor layer is 1050℃ and the growth pressure is 200torr.
[0140] The rest are the same as in Example 1.
[0141] The light emitting diode epitaxial wafers obtained in Examples 1 to 3 and Comparative Example 1 were tested in the following manner:
[0142] The epitaxial wafer was made into a 10 mil×24 mil chip, and its luminous power and operating voltage at 200 mA were tested respectively. The luminous power improvement rate was calculated based on the data of comparative example 1.
[0143] Specifically, the luminous power improvement rate = (luminous power of each embodiment - luminous power of comparative example 1) / luminous power of comparative example 1;
[0144] The specific results are shown in the following table:
[0145]
[0146] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light emitting diode epitaxial wafer, It is characterized in that It comprises a substrate, a buffer layer, an N-type semiconductor layer, a multi-quantum well layer and a P-type semiconductor layer stacked on the substrate in sequence; the P-type semiconductor layer comprises a first composite layer, a second composite layer and a third composite layer stacked on the multi-quantum well layer in sequence; The first composite layer includes a BN layer and a BAs layer sequentially stacked on the multi-quantum well layer. x N 1-x layer; The second composite layer is a periodic structure with a period number of 2 to 10, and each period includes a P-type GaN layer, a BAs y N 1-y Layer and P-type B z Ga 1-z N layers; The third composite layer includes a P-type B sequentially stacked on the second composite layer α Ga 1-α N-layer and P-type InGaN layer; Among them, x>y, z>α.
2. The light emitting diode epitaxial wafer according to claim 1, It is characterized in that The thickness of the BN layer is 10nm to 20nm; and / or The BAs x N 1-x The thickness of the layer is 10nm~20nm, and the value of x ranges from 0.55 to 0.
75.
3. The light emitting diode epitaxial wafer according to claim 1, It is characterized in that The thickness of the P-type GaN layer is 2nm~5nm, and its doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 ; and / or The BAs y N 1-y The thickness of the layer is 2nm~5nm, and the value of y ranges from 0.5 to 0.65; and / or The P-type B z Ga 1-z The thickness of the N layer is 3nm~8nm, and its doping concentration is 1×10 20 cm -3 ~1×10 22 cm -3 , the value range of z is 0.1~0.
3.
4. The light emitting diode epitaxial wafer according to claim 1, It is characterized in that The P-type B α Ga 1-α The thickness of the N layer is 10nm~30nm, and its doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 , the value range of α is 0.05~0.1; and / or The thickness of the P-type InGaN layer is 5nm~20nm, and its doping concentration is 1×10 20 cm -3 ~1×10 22 cm -3 , the In component accounts for 0.1~0.
2.
5. The light emitting diode epitaxial wafer according to any one of claims 1 to 4, It is characterized in that z≤0.2, y≤0.62, so that the BAs y N 1-y The lattice constant of the layer is smaller than that of the P-type B z Ga 1-z Lattice constant of the N layer.
6. The light emitting diode epitaxial wafer according to any one of claims 1 to 4, It is characterized in that The P-type B z Ga 1-z The doping concentration of the N layer is greater than the doping concentration of the P-type GaN layer.
7. The light emitting diode epitaxial wafer according to any one of claims 1 to 4, It is characterized in that The buffer layer is an AlN layer, and its thickness is 30nm-80nm; and / or The N-type semiconductor layer is an N-type GaN layer, and its thickness is 1 μm to 5 μm; and / or The multi-quantum well layer is a periodic structure formed by alternately stacking InGaN quantum well layers and GaN quantum barrier layers, the number of periods is 3 to 15, the thickness of the InGaN quantum well layer is 3nm to 5nm, and the thickness of the GaN quantum barrier layer is 8nm to 15nm.
8. A method for preparing a light emitting diode epitaxial wafer, for preparing the light emitting diode epitaxial wafer as claimed in any one of claims 1 to 7, It is characterized in that include: Providing a substrate, and sequentially growing a buffer layer, an N-type semiconductor layer, a multi-quantum well layer, and a P-type semiconductor layer on the substrate; the P-type semiconductor layer comprises a first composite layer, a second composite layer, and a third composite layer sequentially stacked on the multi-quantum well layer; The first composite layer includes a BN layer and a BAs layer sequentially stacked on the multi-quantum well layer. x N 1-x layer; The second composite layer is a periodic structure with a period number of 2 to 10, and each period includes a P-type GaN layer, a BAs y N 1-y Layer and P-type B z Ga 1-z N layers; The third composite layer includes a P-type B sequentially stacked on the second composite layer α Ga 1-α N-layer and P-type InGaN layer; Among them, x>y, z>α.
9. The method for preparing a light emitting diode epitaxial wafer according to claim 8, It is characterized in that The growth temperature of the BN layer is 1200° C. to 1300° C., and the growth pressure is 50 torr to 200 torr; and / or The BAs x N 1-x The growth temperature of the layer is 850°C to 1000°C and the growth pressure is 100 torr to 300 torr; and / or The growth temperature of the P-type GaN layer is 900° C. to 1100° C., and the growth pressure is 100 torr to 300 torr; and / or The BAs y N 1-y The growth temperature of the layer is 850°C to 1000°C and the growth pressure is 100 torr to 300 torr; and / or The P-type B z Ga 1-z The growth temperature of the N layer is 1000℃~1200℃, and the growth pressure is 100torr~500torr; The P-type B α Ga 1-α The growth temperature of the N layer is 1000°C to 1200°C, and the growth pressure is 100 torr to 500 torr; and / or The growth temperature of the P-type InGaN layer is 800° C. to 900° C., and the growth pressure is 100 torr to 500 torr.
10. A light emitting diode, It is characterized in that It comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Light-emitting diode epitaxial wafer and growth method thereof
CN109920892A
Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode