Cement-based underwater repair material and preparation method thereof

By using acrylamide, initiators and cross-linking agents in cement-based underwater repair materials to form a polymer network structure, combined with anti-scouring agents, the impact and fatigue load resistance of existing underwater concrete repair materials in the underwater environment is solved. It solves the problem of deficiencies, achieves higher impact resistance and erosion resistance, extends the service life of the structure and ensures construction convenience.

CN118684459APending Publication Date: 2024-09-24WUHAN UNIV

Patent Information

Application Number
CN202410805310.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-09-24

AI Technical Summary

Technical Problem

Existing underwater concrete repair materials are easily damaged in the underwater environment, have weak impact and fatigue load resistance, and insufficient tensile and flexural strength and waterproof and anti-corrosion capabilities, resulting in a shortened underwater service life of the structure and an increase in safety hazards.

Method used

The cement-based underwater repair material is used to form a three-dimensional polymer network structure through the polymerization and cross-linking of acrylamide, initiator and cross-linking agent, which enhances the density and adhesion of the material. The anti-erosion agent is used to improve the anti-erosion ability and form a high-quality cement-based underwater repair material. Viscous colloid to resist water erosion.

Benefits of technology

It improves the toughness and impact resistance of underwater repair materials, extends the service life of the structure, enhances the bonding force and erosion resistance to underwater damaged structures, and controls the setting time to ensure the convenience and ease of construction. Material mobility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118684459A
    Figure CN118684459A
Patent Text Reader

Abstract

The invention discloses a cement-based underwater repair material and a preparation method thereof, and relates to the technical field of inorganic nonmetallic materials, and the cement-based underwater repair material is prepared from the following components in parts by weight: 85-94 parts of cement, 4-10 parts of acrylamide, 1.5-3.5 parts of an initiator, 0.01-0.03 part of a cross-linking agent and 0.8-1 part of an anti-scouring agent. The cement-based underwater repair material has the effect of improving the impact resistance of the repair material while improving the binding power of the cement-based underwater repair material to an underwater damaged structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of inorganic non-metallic materials, and in particular to a cement-based underwater repair material and a preparation method thereof. Background Art

[0002] As a non-homogeneous, anisotropic, multi-phase composite material, concrete has a large number of micro-cracks and micro-pores inside. Harmful substances enter the concrete through the pores along with water, causing the internal environment of the concrete to change, resulting in cement degradation and eventual loss of its original strength. When concrete is used in underwater areas, since it needs to be put underwater before the concrete is finalized, the overall structure is loose, and problems such as ion corrosion, water washing away cement and gravel, and long setting time are prominent. With the increase of age, the strength of concrete will show a significant decrease, there will be many pores inside the structure, and it will be easy to crack. This poses a huge hidden danger to the safe use of hydraulic structures, and also greatly limits the service life of the buildings. At present, underwater cracked concrete is often repaired by adjusting the mix ratio, adding special admixtures, and adding organic fiber materials as a repair material, thereby improving the overall density of the material, optimizing the internal structure, reducing moisture intrusion into the concrete, and resisting water erosion, thereby improving its application effect and durability in underwater environments.

[0003] However, since the repair material is still a brittle material, when used in the special underwater environment, the repeated and uninterrupted impact of sand and gravel and the scouring of water will cause its multi-phase structure composed of solid particles, cement slurry, and pores to be destroyed, making its ability to resist impact and fatigue loads weak, and its tensile and flexural strength, as well as its waterproof and corrosion resistance weak. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the related art, the present application provides a cement-based underwater repair material and a preparation method thereof.

[0005] On the one hand, the present application provides a cement-based underwater repair material adopts the following technical solution: A cement-based underwater repair material is made of the following components in parts by weight: 85-94 parts of cement, 4-10 parts of acrylamide, 1.5-3.5 parts of an initiator, 0.01-0.03 parts of a cross-linking agent, and 0.8-1 parts of an anti-scouring agent.

[0006] Preferably, the weight ratio of the cement to the acrylamide is 9-22.5:1.

[0007] Preferably, the weight ratio of the cement to the acrylamide is 11.4:1.

[0008] Preferably, the weight ratio of the acrylamide to the initiator is 2.6-2.7:1.

[0009] Preferably, the weight ratio of the acrylamide to the initiator is 2.66:1.

[0010] Preferably, the weight ratio of the acrylamide to the cross-linking agent is 3-4.2:0.01.

[0011] Preferably, the weight ratio of the acrylamide to the cross-linking agent is 3.89:0.01.

[0012] Preferably, the initiator comprises one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

[0013] Preferably, the initiator is ammonium persulfate.

[0014] Preferably, the cross-linking agent is N,N′-methylenebisacrylamide.

[0015] Preferably, the anti-scour agent is hydroxypropyl methylcellulose.

[0016] On the other hand, the present application provides a cement-based underwater repair material adopting the following technical solution: A method for preparing a cement-based underwater repair material comprises the following steps: taking mixing water and mixing it evenly with the cement, the acrylamide, the initiator, the cross-linking agent and the anti-scour agent to obtain the cement-based underwater repair material.

[0017] Preferably, the method comprises the following steps: uniformly mixing acrylamide, a crosslinking agent and part of the mixing water to obtain a first solution; uniformly mixing an initiator and the remaining mixing water to obtain a second solution; uniformly mixing an anti-scour agent and cement, adding the mixture to the first solution and stirring to obtain a mixed slurry; and uniformly adding the second solution to the mixed slurry and stirring to obtain a cement-based underwater repair material.

[0018] Preferably, after the mixed slurry is prepared, the second solution is added thereto after 10-60 minutes.

[0019] In summary, the present application includes at least one of the following beneficial technical effects: 1. In the present application, when acrylamide, a cross-linking agent and an initiator are polymerized and cross-linked underwater, a uniform three-dimensional polymer network structure is formed inside the cement, and the acrylamide free in the cement voids is also polymerized to produce a highly absorbent polymer hydrogel, which fills the void structure while adsorbing the free water inside the cement, thereby improving the density of the material and retaining water. As the hydration reaction proceeds, water will be gradually released, thereby achieving an internal curing effect and improving the later strength of the material. At the same time, the carboxyl groups formed by the hydrolysis of acrylamide in an alkaline environment bond with the metal ions in the hydration products of the cement, reducing the content of Ca(OH)2 in the matrix, thereby enhancing the interaction between adjacent calcium-silicon layers, strengthening the stability of the interlayer structure, and improving the bonding effect of the produced polyacrylamide and the hydration products, thereby forming a tightly bound organic-inorganic connection structure underwater, jointly bearing stress, and improving the toughness of underwater repair materials. Under the combined effect, the bonding force to the damaged underwater structure is improved, and the impact resistance of the repair material is also improved; 2. Through the cross-linking of acrylamide under the action of initiator and cross-linking agent, a polymer colloid is formed, which improves the expansion of underwater repair materials, improves the filling effect of crack structures, destroys the water layer on the damaged surface, further improves the cohesion inside the material and the adhesion to the damaged structure, and the acrylamide on the surface of the underwater repair material can achieve secondary bonding with the damaged part through water absorption and expansion, metal ion bonding, etc. When damage occurs again. Under the comprehensive effect, the effectiveness and long-term effect of underwater repair are improved; 3. By using anti-scouring agents to form highly viscous colloids in underwater repair materials, the cohesion of cement is enhanced to resist water scouring, but it is also prone to agglomeration, reducing the fluidity of cement. At this time, acrylamide, cross-linking agents and initiators also migrate to various parts of the cement matrix along with water, and some polymer monomers are adsorbed on the surface of cement particles to prevent cement particles from absorbing water. Relying on the charge repulsion effect, the aggregation of particles is reduced, allowing more free water to exist in the pores of cement, so that the underwater repair material can have higher fluidity. Under the combined effect, the anti-scouring ability of the underwater repair material is improved while reducing the fluidity of the underwater repair material as much as possible, which is conducive to construction; 4. In the present application, the initial setting of the underwater repair material is controlled by the polymerization reaction. By adjusting the timing of the introduction of the initiator according to the needs of the project, the setting time of the underwater repair material can be regulated, which is beneficial to the control of the setting time of the underwater repair material during the construction process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope image of a sample obtained by underwater molding of the cement-based underwater repair material of Comparative Example 2 of the present application.

[0021] Figure 2 This is a scanning electron microscope image of a sample obtained by underwater molding of the cement-based underwater repair material of Example 2 of the present application.

[0022] Figure 3 This is a picture of the compressive strength test of the samples obtained by underwater molding of the cement-based underwater repair materials of Example 2 and Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0023] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.

[0024] The raw materials used in the examples and comparative examples can all be obtained commercially.

[0025] Example 1 Example 1 of the present application provides a cement-based underwater repair material, which is prepared by the following steps: 9.22 parts by weight of acrylamide and 0.03 parts by weight of N,N′-methylenebisacrylamide are dissolved in mixing water to obtain a first solution; 3.46 parts by weight of ammonium persulfate are dissolved in mixing water to obtain a second solution; 86.43 parts by weight of cement and 0.86 parts by weight of hydroxypropyl methylcellulose are stirred evenly, and then added to the first solution to obtain a mixed slurry, and the mixed slurry and the second solution are stirred with a slurry mixer until they are evenly mixed to obtain a cement-based underwater repair material.

[0026] Example 2 Example 2 of the present application provides a cement-based underwater repair material. The difference between Example 2 and Example 1 is that in Example 2, the amount of acrylamide used is 7.78 parts by weight, the amount of N,N′-methylenebisacrylamide used is 0.02 parts by weight, the amount of ammonium persulfate used is 2.92 parts by weight, the amount of cement used is 88.40 parts by weight, and the amount of hydroxypropyl methylcellulose used is 0.88 parts by weight.

[0027] Example 3 Example 3 of the present application provides a cement-based underwater repair material. The difference between Example 3 and Example 1 is that in Example 3, the amount of acrylamide used is 4.15 parts by weight, the amount of N,N′-methylenebisacrylamide used is 0.01 parts by weight, the amount of ammonium persulfate used is 1.56 parts by weight, the amount of cement used is 93.35 parts by weight, and the amount of hydroxypropyl methylcellulose used is 0.93 parts by weight.

[0028] Example 4 Example 4 of the present application provides a cement-based underwater repair material, which is prepared by the following steps: 7.78 parts by weight of acrylamide and 0.02 parts by weight of N,N′-methylenebisacrylamide are dissolved in mixing water to obtain a first solution; 2.92 parts by weight of ammonium persulfate are dissolved in mixing water to obtain a second solution; 88.40 parts by weight of cement and 0.88 parts by weight of hydroxypropyl methylcellulose are stirred evenly, and then added to the first solution to obtain a mixed slurry. After 10 minutes, the mixed slurry and the second solution are stirred with a slurry mixer until they are evenly mixed to obtain a cement-based underwater repair material.

[0029] Example 5 Example 5 of the present application provides a cement-based underwater repair material, which is prepared by the following steps: 7.78 parts by weight of acrylamide and 0.02 parts by weight of N,N′-methylenebisacrylamide are dissolved in mixing water to obtain a first solution; 2.92 parts by weight of ammonium persulfate are dissolved in mixing water to obtain a second solution; 88.40 parts by weight of cement and 0.88 parts by weight of hydroxypropyl methylcellulose are stirred evenly, and then added to the first solution to obtain a mixed slurry. After 30 minutes, the mixed slurry and the second solution are stirred with a slurry mixer until they are evenly mixed to obtain a cement-based underwater repair material. Example 6 Example 6 of the present application provides a cement-based underwater repair material, which is prepared by the following steps: 7.78 parts by weight of acrylamide and 0.02 parts by weight of N,N′-methylenebisacrylamide are dissolved in mixing water to obtain a first solution; 2.92 parts by weight of ammonium persulfate are dissolved in mixing water to obtain a second solution; 88.40 parts by weight of cement and 0.88 parts by weight of hydroxypropyl methylcellulose are stirred evenly, and then added to the first solution to obtain a mixed slurry. After 60 minutes, the mixed slurry and the second solution are stirred with a slurry mixer until they are evenly mixed to obtain a cement-based underwater repair material.

[0030] Comparative Example 1 Comparative Example 1 of the present application provides a cement-based underwater repair material, which is prepared by the following steps: 11.17 parts by weight of acrylamide and 0.03 parts by weight of N,N′-methylenebisacrylamide are dissolved in mixing water to obtain a first solution; 4.19 parts by weight of ammonium persulfate are dissolved in mixing water to obtain a second solution; 83.77 parts by weight of cement and 0.84 parts by weight of hydroxypropyl methylcellulose are stirred evenly, then added to the first solution and stirred to obtain a mixed slurry, and the mixed slurry and the second solution are stirred with a slurry mixer until they are evenly mixed to obtain a cement-based underwater repair material.

[0031] Comparative Example 2 Comparative Example 2 of the present application provides a cement-based underwater repair material, which is prepared by the following steps: 99 parts by weight of cement, 1 part by weight of hydroxypropyl methylcellulose and mixing water are stirred in a slurry mixer until the mixture is uniform to obtain a cement-based underwater repair material.

[0032] Test and Inspection (1) According to the standard DL / T 5117-2021 "Test Procedure for Underwater Non-dispersible Concrete", the cement-based underwater repair materials of Examples 1-3 and Comparative Examples 1-2 were underwater molded to obtain samples of bonding strength, flexural strength, compressive strength, anti-dispersion, and fluidity tests. The test results are shown in Tables 1 and 2.

[0033] Table 1:

[0034] Table 2:

[0035] (2) Scanning electron microscope imaging was performed on the sample obtained by underwater molding of the cement-based underwater repair material of Comparative Example 1, as shown in FIG. Figure 1 shown.

[0036] (3) Scanning electron microscope imaging was performed on the sample obtained by underwater molding of the cement-based underwater repair material of Example 2, as shown in FIG. Figure 2 shown.

[0037] (4) According to the standard "Standard Test Method for Cement", the flexural strength and bonding strength of the cement-based underwater repair materials of Examples 1-3 and Comparative Examples 1-2 were tested for the above-water molded specimens. The test results are shown in Table 3.

[0038] Table 3:

[0039] (5) According to JGT 3420-2020 "Testing Procedures for Cement and Cement Concrete for Highway Engineering", the initial setting time and final setting time of Example 2 and Examples 4-6 were tested (the initial setting time and final setting time were calculated based on the time when cement was added and mixed to obtain the mixed slurry). As shown in Table 4.

[0040] Table 4:

[0041] Results Analysis The present application is described in detail below in conjunction with the experimental data provided in Tables 1-4.

[0042] Reference Figure 1 ,in Figure 1 -a is 5000 times magnification, Figure 1 -b is magnified 15000 times. The sample obtained by underwater molding of the cement-based underwater repair material of comparative example 2 has a large number of pore structures, a large number of cluster structures are widely distributed on the surface, and there is obvious aggregation around the holes. In addition, there are a large number of micropores and microcracks in the microstructure. The overall structure is loose, the porosity is large, and the connection between the crystals is weak. Figure 2 ,in Figure 2 -a is 5000 times magnification, Figure 2 -b is a magnification of 15,000 times. The surface microstructure of the sample obtained by underwater molding of the cement-based underwater repair material in Example 2 is more compact, the large pores are filled into small pores, the connection between the crystals is closer, and the crystal structure is transformed from a brittle and easily broken rod-like structure to a flat structure. The pore volume is significantly reduced, and the number of large pores is reduced.

[0043] Reference Figure 3 ,in Figure 3 -a is a sample obtained by underwater molding of the cement-based underwater repair material of Comparative Example 2, Figure 3 -b is the sample obtained by underwater molding of the cement-based underwater repair material of Example 2. The sample obtained by underwater molding of the cement-based underwater repair material of Example 2 had only tiny cracks on the surface after the compressive strength test, while the sample obtained by underwater molding of the cement-based underwater repair material of Comparative Example 2 had block shedding on the surface after the compressive strength test and formed large cracks that penetrated the material.

[0044] With reference to Examples 1-3 and Comparative Examples 1-2, the data in Table 1 show the effects of different amounts of acrylamide added on the bonding strength, flexural strength, compressive strength, anti-scouring and fluidity of the prepared cement-based underwater repair materials during underwater molding. Among them, when the cement-based underwater repair materials of Examples 1-3 are molded underwater, the bonding strength, flexural strength and compressive strength are all higher than the various strengths of the cement-based underwater repair materials of Comparative Example 2, and when the cement-based underwater repair materials of Example 2 are molded underwater, the bonding strength, flexural strength and compressive strength are also higher than the various strengths of the cement-based underwater repair materials of Examples 1 and 3. Analysis is due to the addition of polymer components of acrylamide, initiator and cross-linking agent to form a complementary effect with rigid, high-strength inorganic cement-based materials, which is conducive to improving the various strengths of cement-based underwater repair materials. However, when the amount of acrylamide added is too large, it will directly affect the strength development of the material. As shown in the data of Comparative Example 1 in Table 1, although the bonding strength is improved, the flexural strength and compressive strength are both reduced. When the anti-dispersion performance is verified by the suspended matter content determination method specified in DL / T 5117-2021 "Test Procedure for Underwater Non-dispersible Concrete", the suspended matter content of the cement-based underwater repair materials in Examples 1-3 during the underwater molding process increases successively, but is much less than the suspended matter content of Comparative Example 2. Analysis shows that the presence of acrylamide effectively enhances the use effect of the anti-scouring agent in Comparative Example 2, hinders the diffusion of cement particles when the material enters the water, thereby improving the underwater anti-dispersion ability of the material. This effect weakens as the acrylamide content decreases. The fluidity of the cement-based underwater repair materials in Examples 1-3 during the underwater molding process decreases successively, but is always greater than that of Comparative Example 2. The excellent fluidity ensures the uniformity of the entire material, reduces the difficulty of mixing, and effectively guarantees the quality of construction and pouring. In addition, during the repair process, the cement-based underwater repair material can also effectively fill the cracks in the matrix and reduce pores.

[0045] Comparing the data of bonding strength and flexural strength in Table 1, Table 2 and Table 3, it is shown that the different molding environments of the cement-based underwater repair materials of Examples 1-3 and Comparative Examples 1-2 during water molding and underwater molding affect the bonding strength and flexural strength. The bonding strength of the samples obtained under underwater molding conditions of the cement-based underwater repair materials of Examples 1-3 is higher than the bonding strength of the samples obtained under underwater molding conditions of the cement-based underwater repair materials of Comparative Examples 1-2. The analysis is mainly due to the fact that acrylamide can be adsorbed on the cement surface before reacting to reduce the consistency, and the polymer gel formed after the reaction has a certain viscosity and can fill the pores, thereby improving the bonding properties of the material. In addition, during the normal underwater repair process, due to the presence of a water layer on the surface of the substrate to be repaired, it will directly affect the underwater repair effect and hinder the bonding of the repair material. The polymer formed during the use of the cement-based underwater repair materials of Examples 1-3 has a certain water absorption capacity, which can directly destroy the water layer, ensure close bonding with the damaged substrate, and further improve the bonding strength of the material. When the curing age is 28 days, the flexural strength of the samples of the cement-based underwater repair materials of Examples 1-3 obtained under underwater molding conditions is generally higher than the flexural strength of the samples of the cement-based underwater repair materials of Examples 1-3 obtained under water molding conditions. Analysis shows that this is because cement itself is a high-strength brittle material, while the polymer gel produced by the cement-based underwater repair materials of Examples 1-3 during use is a high-elastic and tough material. Under underwater conditions, the gel absorbs water to saturate, expands in volume, occupies more volume, and the overall structure is more tough. At the same time, the strength of cement is also developed to a certain extent under long-term curing. In summary, the flexural strength is significantly improved. In particular, the 28-day bonding strength and flexural strength of the sample obtained by the cement-based underwater repair material of Example 2 under underwater molding conditions are higher than the 28-day bonding strength and flexural strength of the sample obtained by the cement-based underwater repair material of Example 2 under water molding conditions, indicating that acrylamide is more suitable for underwater repair in terms of improving the 28-day bonding strength and flexural strength when used in an appropriate amount. Analysis is due to the fact that the cement-based underwater repair material of Example 2 has a suitable amount of acrylamide, which fully utilizes the high viscosity of the polymer colloid, and the gel is always in a saturated state underwater, so the bonding strength is improved.

[0046] Referring to Table 4, Example 2 and Examples 4-6 show the effect of the timing of adding the initiator on the initial setting time and the final setting time. It can be found that the cement-based underwater repair materials of Example 2 and Examples 4-6 can complete the initial setting in 4 to 6 minutes after adding the initiator, and complete the final setting in 10-15 minutes. That is, in the actual engineering construction process, the setting time of the cement-based underwater repair material can be adjusted by the timing of adding the initiator.

[0047] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A cement-based underwater repair material, characterized in that: The invention is prepared from the following components in parts by weight: 85-94 parts of cement, 4-10 parts of acrylamide, 1.5-3.5 parts of initiator, 0.01-0.03 parts of cross-linking agent and 0.8-1 parts of anti-scour agent.

2. The cement-based underwater repair material according to claim 1, characterized in that: The weight ratio of the cement to the acrylamide is 9-22.5:

1.

3. The cement-based underwater repair material according to claim 1, characterized in that: The weight ratio of the acrylamide to the initiator is 2.6-2.7:

1.

4. The cement-based underwater repair material according to claim 1, characterized in that: The weight ratio of the acrylamide to the cross-linking agent is 3-4.2:0.

01.

5. The cement-based underwater repair material according to claim 1, characterized in that: The initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

6. The cement-based underwater repair material according to claim 1, characterized in that: The cross-linking agent is N,N'-methylenebisacrylamide.

7. The cement-based underwater repair material according to claim 1, characterized in that: The anti-scour agent is hydroxypropyl methylcellulose.

8. A method for preparing a cement-based underwater repair material according to any one of claims 1 to 7, characterized in that: The following steps are involved: The mixing water is mixed evenly with the cement, the acrylamide, the initiator, the cross-linking agent and the anti-scour agent to obtain a cement-based underwater repair material.

9. The method for preparing a cement-based underwater repair material according to claim 8, characterized in that: The following steps are involved: uniformly mixing acrylamide, a cross-linking agent and a portion of mixing water to obtain a first solution; The initiator is mixed evenly with the remaining mixing water to obtain a second solution; the anti-scour agent and cement are mixed evenly and then added to the first solution and stirred evenly to obtain a mixed slurry; The second solution is added into the mixed slurry and stirred evenly to obtain a cement-based underwater repair material.

10. The method for preparing a cement-based underwater repair material according to claim 9, characterized in that: After the mixed slurry is prepared, the second solution is added thereto after 10-60 minutes.

Citation Information

Patent Citations

  • Concrete for underwater engineering and preparation method thereof

    CN111517727A

  • Quick-setting adjustable cement-based underwater anti-dispersion ultrafast-hardening grouting material as well as preparation method and application thereof

    CN111777389A

  • High-toughness cement-based material as well as preparation method and application thereof

    CN116854430A

  • Cement-based material for realizing underwater 3D printing through in-situ graft polymerization and preparation method of cement-based material

    CN117447133A

  • Grout material for underwater application

    JP2007261921A

Cited By

  • Hydrogel-cement-based composite grouting material capable of being used underwater

    CN119774941A

  • A hydrogel-cement-based composite grouting material suitable for use in dynamic underwater environments

    CN119774941B

  • Composite repairing material for underwater defects of ultra-deep concrete diaphragm wall and targeted repairing method

    CN120829293A

  • Cement-based composite performance evaluation system and method based on multi-source data analysis

    CN121215138A