Functionalized polyurethane, meniscus prosthesis, preparation method and use thereof
By using functionalized polyurethane materials in meniscal prostheses, combined with self-healing polyurethane elastomers and adamantane-hyaluronic acid composites, the low mechanical properties and wear problems of meniscal substitutes are solved, and self-lubrication and self-healing are achieved. function, extending the material life and protecting articular cartilage, providing a new treatment option for meniscal injuries.
Patent Information
- Application Number
- CN202411177632.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing meniscal substitutes have problems such as low mechanical properties, severe wear, easy degradation, and short service life, and cannot well adapt to the dynamic self-repairing ability and physiological cyclic lubrication mechanism of natural meniscus.
Functionalized polyurethane material is used, combined with self-healing polyurethane elastomer and adamantane-hyaluronic acid compound. By evenly covering the adamantane-hyaluronic acid compound on the surface of the polyurethane elastomer, a self-lubricating and self-healing polyurethane material is formed, simulating natural The dynamic self-healing ability of the meniscus and the physiological circulatory lubrication mechanism.
It achieves high modulus, high elasticity, and low friction coefficient, prolongs the life of the material, protects articular cartilage, slows down the progression of osteoarthritis, and provides an effective treatment plan for meniscal injuries.
Smart Images

Figure CN118697939B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and in particular relates to a functionalized polyurethane, a meniscus prosthesis, and a preparation method and application thereof. Background Art
[0002] The precise anatomical structure of the meniscus is crucial for the complex movement and stable support of the knee joint. In clinical practice, total meniscectomy is still the preferred treatment for irreparable meniscus injury and severe meniscus degeneration; however, this will inevitably lead to knee joint stability disorder, articular cartilage wear, and ultimately the formation of osteoarthritis. In order to solve this problem, a series of meniscus substitutes have been developed. The geometric features of most meniscus replacements cannot be well matched with the natural meniscus and cannot restore the initial stress distribution in the joint compartment; secondly, although most constructed tissue engineering meniscus materials have a compression modulus similar to that of the natural meniscus, the tensile modulus is far from the circumferential / radial tensile modulus of the natural meniscus, which does not match the anisotropic mechanical characteristics of the natural meniscus. When subjected to load, large deformation will occur due to circumferential expansion, causing local collapse and fracture of the meniscus scaffold. In addition, repeated contact and friction between the femur and tibia on the meniscus also leads to severe wear of the tissue engineering meniscus. Since the knee joint cavity is rich in synovial fluid and proteases, the rapid degradation of meniscus materials after implantation in the body is also one of the current disadvantages.
[0003] Polyurethane elastomers are a type of polymer material with unique properties. They combine the elasticity of rubber and the durability of plastic, and have excellent tensile strength, tear strength and impact resistance. These properties enable them to perform well under heavy pressure and impact, especially in high-friction environments. In addition, due to the excellent biocompatibility of polyurethanes, they have been used in the medical field, such as making artificial blood vessels, pacemakers and artificial bones.
[0004] Self-healing material is a new type of intelligent material that can repair its mechanical damage and restore its original function under certain external stimuli. It relies on reversible forces such as reversible covalent bonds or non-covalent bonds. Under the influence of external stimuli, it can achieve the purpose of completely restoring its performance through reversible fracture and generation. Theoretically, it can achieve an unlimited number of repair times.
[0005] The lubrication of articular cartilage and meniscus is crucial in knee joint movement. Hyaluronic acid and lubricin in synovial fluid are the main lubricating components. The knee joint is subjected to extremely complex and demanding loads in daily activities. Even under high loads, the friction coefficient of articular cartilage in the knee joint is as low as 10 -3Based on the physiological lubrication phenomenon of the knee joint, tissue engineering meniscus / cartilage scaffolds with self-lubricating function, thereby increasing the material life and delaying the progression of osteoarthritis, has become one of the current research hotspots.
[0006] At present, meniscus substitutes have problems such as low mechanical properties, severe wear, easy degradation, short service life, and poor compatibility with natural meniscus. Therefore, it is urgent to develop a new type of meniscus prosthesis that simulates the dynamic self-repair ability and physiological circulation lubrication mechanism of the natural meniscus, and provides a new solution for the treatment of meniscus injuries. Summary of the invention
[0007] In view of the problems in the prior art, the present invention provides a functionalized polyurethane, a meniscus prosthesis and a preparation method and use thereof.
[0008] A functionalized polyurethane, characterized in that it comprises a self-repairing polyurethane elastomer and an adamantane-hyaluronic acid complex, wherein the adamantane-hyaluronic acid complex is covered on the surface of the self-repairing polyurethane elastomer, and the thickness of the adamantane-hyaluronic acid complex is 10-20 microns;
[0009] The self-repairing polyurethane elastomer is made of the following raw materials in parts by weight:
[0010] 1-2 parts of hard segment raw materials,
[0011] Soft segment raw material 4.5-9 parts,
[0012] 0.262-0.522 parts of dimethylglyoxime,
[0013] Chain extender 0.412-0.824 parts,
[0014] Cross-linking agent 0.04-0.08 parts;
[0015] The adamantane-hyaluronic acid complex is made of the following raw materials in parts by weight:
[0016] 10-20 parts of hyaluronic acid,
[0017] 2.3-4.6 parts of diepoxide,
[0018] 0.5~5 parts of adamantane.
[0019] Preferably, the self-repairing polyurethane elastomer is made of the following raw materials in parts by weight:
[0020] 1 part of hard segment raw material,
[0021] 4.5 parts of soft segment raw material,
[0022] 0.262-0.522 parts of dimethylglyoxime,
[0023] Chain extender 0.412 parts,
[0024] Crosslinking agent 0.04 parts.
[0025] Preferably, the self-repairing polyurethane elastomer is made of the following raw materials in parts by weight:
[0026] 1 part of hard segment raw material,
[0027] 4.5 parts of soft segment raw material,
[0028] 0.392 parts of dimethylglyoxime,
[0029] Chain extender 0.412 parts,
[0030] Crosslinking agent 0.04 parts.
[0031] Preferably, the adamantane-hyaluronic acid complex is made from the following raw materials in parts by weight:
[0032] Hyaluronic acid 10 parts,
[0033] 2.3 parts of diepoxide,
[0034] Adamantane 0.5-5 parts.
[0035] Preferably, the adamantane-hyaluronic acid complex is made from the following raw materials in parts by weight:
[0036] Hyaluronic acid 10 parts,
[0037] 2.3 parts of diepoxide,
[0038] Adamantane 5 parts.
[0039] Preferably, the hard segment raw material is selected from at least one of isophorone diisocyanate and polycaprolactone triol;
[0040] And / or, the soft segment raw material is selected from at least one of polytetramethylene ether and polypropylene oxide;
[0041] And / or, the chain extender is selected from at least one of 1,4-butanediol and glycerol;
[0042] And / or, the cross-linking agent is selected from at least one of aminocyclodextrin and ethylenediamine;
[0043] And / or, the diepoxy compound is selected from at least one of 1,4-butanediol diglycidyl ether and 1,6-hexanediol diglycidyl ether.
[0044] The present invention also provides a method for preparing the functionalized polyurethane, comprising the following steps:
[0045] Step 1, reacting a hard segment raw material and a soft segment raw material to obtain a mixture A;
[0046] Step 2, reacting mixture A with dimethylglyoxime to obtain mixture B;
[0047] Step 3, reacting the mixture B with a chain extender and a crosslinker, and obtaining a self-repairing polyurethane elastomer after purification;
[0048] Step 4, reacting hyaluronic acid with a diepoxide compound to obtain a mixture C;
[0049] Step 5, reacting the mixture C with adamantane to obtain an adamantane-hyaluronic acid complex;
[0050] Step 6, uniformly covering the surface of the self-repairing polyurethane elastomer with the adamantane-hyaluronic acid complex to obtain a self-lubricating-self-repairing polyurethane elastomer material.
[0051] Preferably, in step 1, the reaction temperature is 60-80°C and the reaction time is 45 min-1.5 h;
[0052] And / or, in step 2, the reaction temperature is 60-80°C and the reaction time is 1-2 h;
[0053] and / or, in step 3, the reaction temperature is 60-80°C and the reaction time is 0.5-2 h;
[0054] and / or, in step 4, the reaction temperature is 20-50°C and the reaction time is 6-12 h;
[0055] And / or, in step 5, the reaction temperature is 40-80° C., and the reaction time is 12-36 h.
[0056] The present invention also provides use of the functionalized polyurethane in preparing a meniscus prosthesis.
[0057] The invention also provides a meniscus prosthesis, which is made of the functionalized polyurethane.
[0058] The present invention designs a polyurethane meniscus prosthesis with self-lubricating and self-repairing functions. The meniscus prosthesis uses polyurethane as a substrate, introduces a self-repairing chemical bond - a dynamic dimethylglyoxime-carbamate group, and then introduces an adamantane structure on the surface of the self-repairing polyurethane elastomer to carry hyaluronic acid. It has high modulus, high elasticity, and high lubrication properties, and at the same time exhibits good biocompatibility and cartilage protection, providing a new solution for the treatment of meniscus injuries.
[0059] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0060] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 Schematic diagram of the self-repair test of the self-repairing polyurethane meniscus main material.
[0062] Figure 2 This is a graph of the tensile properties of the polyurethane meniscus material, where a is the self-healing efficiency of the self-healing polyurethane elastomer, b is the tensile modulus of the self-healing polyurethane elastomer, c is the ultimate tensile strength of the self-healing polyurethane elastomer, and d is the tensile stress of DPU2-CD.
[0063] Figure 3 This is the compression performance result diagram of the polyurethane meniscus material, where a is the compression modulus of the self-healing polyurethane elastomer and b is the compressive stress of DPU2-CD.
[0064] Figure 4 This is the test result of the friction coefficient of the polyurethane meniscus.
[0065] Figure 5 Figures 1 and 2 are the results of biocompatibility test of polyurethane meniscus, where a and f are the evaluation of cell activity of different material groups using live-dead staining method and the quantitative results, b, e, g are the effects of different material groups on chondrocyte proliferation evaluated by EDU labeling and CCK-8 method, and c and d are the evaluation of cell migration ability of different material groups using scratch test and Transwell chamber test.
[0066] Figure 6 Immunofluorescence technology was used to evaluate the effects of materials on the expression of chondrocyte synthesis and decomposition proteins, where a and d are the expression and quantitative results of the anabolic protein COL-2, and b and c are the expression and quantitative results of the decomposition protein MMP-13.
[0067] Figure 7 A polyurethane meniscus prosthesis is placed in a rabbit.
[0068] Figure 8At 6 weeks and 12 weeks after surgery, the knee cartilage of the femoral condyle, femoral trochlea, and tibial plateau of the three groups of rabbits were grossly observed and evaluated by Micro CT scanning to quantitatively and qualitatively analyze the protective effect on the knee cartilage. Among them, a is the gross image of the femoral condyle of the three groups at 6 weeks and 12 weeks after surgery, b is the gross image of the femoral trochlea of the three groups at 6 weeks and 12 weeks after surgery, c is the gross image of the tibial plateau of the three groups at 6 weeks and 12 weeks after surgery, d is the Micro CT image of the three groups at 6 weeks after surgery, e is the Micro CT image of the three groups at 12 weeks after surgery, f is the quantitative image of the gross cartilage score at 6 weeks and 12 weeks after surgery, g is the quantitative evaluation image of the knee osteophyte volume at 6 weeks and 12 weeks after surgery, and h is the quantitative evaluation image of the subchondral bone density of the three groups at 6 weeks and 12 weeks after surgery.
[0069] Fig. 9 Figure 3 shows the results of femtosecond laser detection of articular cartilage, where a is the collagen and metabolite evaluation graph of the subtotal resection group 6 and 12 weeks after surgery, b is the collagen and metabolite evaluation graph of the PU group 6 and 12 weeks after surgery, c is the collagen and metabolite evaluation graph of the DPU@HA group 6 and 12 weeks after surgery, and d is the collagen and metabolite evaluation graph of natural articular cartilage 6 and 12 weeks after surgery. DETAILED DESCRIPTION
[0070] In the following examples and experimental examples, reagents and raw materials not specifically described are all commercially available products.
[0071] Example 1: Preparation of self-lubricating and self-repairing polyurethane elastomer meniscus prosthesis
[0072] This embodiment provides a self-lubricating and self-repairing polyurethane elastomer meniscus prosthesis, and the preparation method thereof is as follows:
[0073] 1. Synthesis of self-healing polyurethane elastomer (DPU-CD)
[0074] Under nitrogen protection, first add 5 grams of isophorone diisocyanate (IPDI, Aladdin, CAS 4098-71-9) to a three-necked flask containing 15 milliliters of toluene. Then, add 22.5 grams of polytetramethylenetetramethylene ether (PTMG, Aladdin, CAS 25190-06-1) with a molar ratio of 1:1 to IPDI, and heat and stir at 60°C for 60 minutes to form a basic prepolymer. Then, according to different self-healing performance requirements, slowly add the following amount of dimethylglyoxime (DMG),
[0075] DPU1: 1.31 g of DMG was added at a molar ratio of 1:1 with IPDI to introduce self-healing properties to a moderate degree;
[0076] DPU2: 1.96 g of DMG was added, with a molar ratio of 1.5:1 to IPDI to introduce self-healing properties to a higher degree;
[0077] DPU3: 2.61 g of DMG was added in a molar ratio of 2:1 to IPDI to introduce self-healing properties to the highest degree. In each case, 2.06 g of 1,4-butanediol (BDO, Aladdin, CAS 110-63-4) was then slowly added and the reaction continued at 60 degrees Celsius for 60 minutes to carry out a chain extension reaction to form a polyurethane prepolymer. After that, 0.2 g of aminocyclodextrin (CD, Aladdin, CAS 29390-67-8) was added and the reaction continued at 60°C for 2 h. After the reaction was completed, the mixture was poured into acetone at room temperature to dissolve, and then precipitated in cyclohexane to obtain a white solid precipitate. The precipitate was filtered, washed with cyclohexane, and finally dried under reduced pressure at room temperature for 5 hours to obtain self-healing polyurethane elastomer white powder DPU1-CD, DPU2-CD, and DPU3-CD.
[0078] 2. Preparation of adamantane-hyaluronic acid complex (AD-HA)
[0079] First, 10 g of hyaluronic acid (HA) was reacted with 2.3 g of 1,4-butanediol diglycidyl ether (as a representative of diepoxy compounds) at 50 ° C. The reaction lasted for 12 h to allow uniform mixing. After the reaction was completed, the unreacted 1,4-butanediol diglycidyl ether and by-products were removed by dialysis to obtain an epoxy modified HA solution. Subsequently, the solution containing the epoxy modified HA derivative was pre-frozen at -20 ° C for about 2 h, and then placed in a freeze dryer for a primary drying under a low pressure environment of 0.1 mbar, with the temperature controlled at about -20 ° C for 8 hours to promote the sublimation of ice crystals; followed by a secondary drying, and continued drying at a pressure of 0.01 mbar and a temperature of 20 ° C for 4 hours to remove residual moisture, and finally a loose and porous solid epoxy modified HA derivative was obtained.
[0080] Next, the obtained epoxy modified HA derivative was reacted with adamantane at 80°C for 24 h to prepare an adamantane-hyaluronic acid (AD-HA) complex. The amount of adamantane used is determined according to the molar ratio of the epoxy group in the epoxy modified HA, and this ratio can usually be set to 1:1 to 1:10. If the molar ratio is 1:1, 5 grams of adamantane is used in an amount equal to that of the epoxy modified HA derivative; if the molar ratio is 1:10, 0.5 grams of adamantane is used to adjust the lubricity and mechanical strength of the complex. Finally, the pure adamantane-hyaluronic acid complex (AD-HA) is obtained by filtration and washing.
[0081] 3. Synthesis of self-lubricating and self-repairing polyurethane elastomer meniscus material (DPU-CD+AD-HA)
[0082] First, accurately weigh 20 g of self-healing polyurethane elastomer powder (DPU-CD) and dissolve it in 50 mL of acetone. Use a magnetic stirrer to stir thoroughly at room temperature (about 25°C) until the powder is completely dissolved to form a uniform solution. Subsequently, pour the solution into a pre-cleaned and treated flat polyester film mold, and use a scraper to ensure that the solution evenly covers the entire mold surface to avoid the formation of bubbles or uneven thickness. Next, place the mold containing the polyurethane solution in an oven preheated to 40°C. The drying process lasts for about 3 hours until the acetone is completely evaporated to form a uniform and continuous polyurethane film.
[0083] Subsequently, a lubricating coating of adamantane-hyaluronic acid complex (AD-HA) was prepared. 5 g of the complex powder was dispersed in 10 ml of deionized water and an ultrasonic bath was used for 10 minutes to form a uniform coating solution. Then, a soft brush or a scraper was used to evenly apply the coating on the surface of the formed polyurethane film to ensure the uniformity and consistency of the coating. The coating thickness was controlled within the range of 10-20 μm, and the specific coating thickness in this embodiment was 15 μm.
[0084] 4. Preparation of self-lubricating and self-repairing polyurethane elastomer meniscus prosthesis
[0085] After the coating is completed, the real meniscus is reconstructed in three dimensions using CT images and CAD software to obtain its precise geometric shape and size information, design a digital model of the meniscus prosthesis, and use stereolithography (SLA) high-precision 3D printing technology to make the corresponding mold. Photocurable resin is selected as the 3D printing material to ensure the accuracy and complexity of the mold. The print nozzle diameter is 50 μm and the printing platform temperature is 25°C. Finally, thermoplastic polyurethane material is used to construct a meniscus prosthesis with self-repairing and self-lubricating properties through a reverse molding process. Thermoplastic polyurethane particles are melted at 180°C and poured into the 3D printed mold. A pressure of 50 Pa is applied and maintained at this temperature for 2 minutes to ensure that the material fills the mold evenly. After the molded meniscus prosthesis is taken out, post-processing is performed, including curing at room temperature for 24 hours to improve mechanical properties, and surface treatment with fine sandpaper to obtain the desired finish.
[0086] Example 2: Self-lubricating and self-repairing polyurethane elastomer meniscus prosthesis 2
[0087] The sample is made of 10 grams of isophorone diisocyanate, 22.5 grams of polytetramethylene oxide, 1.31 grams of dimethylglyoxime, 4.12 grams of 1,4-butanediol, 0.2 grams of aminocyclodextrin, 20 grams of hyaluronic acid, 2.3 grams of 1,4-butanediol diglycidyl ether, and 5 grams of adamantane. Except for the different raw material usage ratios, the preparation method is the same as that in Example 1.
[0088] Example 3: Self-lubricating and self-repairing polyurethane elastomer meniscus prosthesis 3
[0089] The sample is made of 5 grams of isophorone diisocyanate, 45 grams of polytetramethylene oxide, 2.61 grams of dimethylglyoxime, 2.06 grams of 1,4-butanediol, 0.4 grams of aminocyclodextrin, 10 grams of hyaluronic acid, 4.6 grams of 1,4-butanediol diglycidyl ether, and 0.5 grams of adamantane. Except for the different raw material usage ratios, the preparation method is the same as that in Example 1.
[0090] Comparative Example 1
[0091] This comparative example provides the control samples used in the experiment:
[0092] 1. PU
[0093] Under nitrogen protection, 5 g of isophorone diisocyanate (IPDI, Aladdin, CAS 4098-71-9) was first added to a three-necked flask containing 15 ml of toluene. Subsequently, 22.55 g of polytetramethylene glycol (PTMG, Aladdin, CAS 25190-06-1) was added at a molar ratio of 1:1 to IPDI, and heated and stirred at 60 degrees Celsius for 60 minutes to form a basic prepolymer. Then, 2.06 g of 1,4-butanediol (BDO, Aladdin, CAS 110-63-4) was slowly added, and the reaction continued at 60 degrees Celsius for 60 minutes to carry out a chain extension reaction to form a polyurethane prepolymer. After the reaction was completed, the mixture was poured into acetone at room temperature to dissolve, and then precipitated in cyclohexane to obtain a white solid precipitate. The precipitate was filtered, washed with cyclohexane, and finally dried under reduced pressure at room temperature for 5 hours to obtain pure polyurethane white powder (PU).
[0094] 2. Self-healing polyurethane elastomer (DPU-CD)
[0095] The sample is composed of isophorone diisocyanate, polytetramethylene oxide, dimethylglyoxime, 1,4-butanediol and aminocyclodextrin, and its preparation method and raw material dosage ratio are the same as those in step 1 of Example 1.
[0096] The technical solution of the present invention is further illustrated by experiments below. The samples used in the experiments are prepared according to the method of Example 1.
[0097] Experimental Example 1: Performance test of self-lubricating and self-repairing polyurethane meniscus material
[0098] The DPU-CD+AD-HA, DPU-CD, and PU samples used in this experimental example were all prepared according to the method of Example 1 or Comparative Example 1.
[0099] 1. Experimental Methods
[0100] Self-healing test: After synthesizing the self-healing polyurethane (DPU-CD), use a cutter to evenly divide the DPU-CD into two parts, one in red and the other in blue. When dried at room temperature at 37°C, the two parts are placed in contact with each other. After 2 minutes, the two parts are pulled to determine whether they can heal themselves.
[0101] Mechanical properties test: The mechanical properties of polyurethane materials with different compositions were tested using an electronic universal testing machine (Instron, USA). In order to characterize the tensile properties of polyurethanes with different compositions, rectangular splines with a length of 40 mm, a width of 5 mm, and a thickness of 0.8 mm were constructed, and tensile tests were performed on them (tensile rate: 50 mm / min). In order to characterize the compressive properties of polyurethane materials, a polyurethane cylindrical structure with a diameter of 10 mm and a thickness of 2.5 mm was constructed in this work, and compression tests were performed on it (compression rate: 10 mm / min). The cyclic tensile setting was 10% deformation, 50 times, and the cyclic compression setting was 20% deformation, 50 times.
[0102] Friction performance test: After selecting the best DPU-CD based on the previous mechanical properties, a supramolecular coating was added to construct DPU-CD+AD-HA. DPU-CD and PU were used as control samples. The friction test of the material was carried out using a universal friction reciprocating tester. The oscillation amplitude, frequency, applied load and test time were 4 mm, 1 Hz, 1 N and 600 s respectively. The COF measurement started 0.495 seconds after the start of oscillation, and the data was recorded at intervals of 1 second.
[0103] 2. Experimental Results
[0104] The self-healing test results are as follows Figure 1 As shown, DPU-CD healed itself within 2 min.
[0105] The tensile properties test results are as follows Figure 2 As shown in ad, DPU2-CD has the highest tensile modulus compared to other groups while having self-repair efficiency, which has exceeded the level of natural meniscus circumferential tensile modulus, indicating that the internal structure of this meniscus substitute can provide sufficient tensile performance. Figure 3 As shown in ab, DPU2-CD has the highest compression modulus compared to other groups while having self-repair efficiency, so DPU2-CD was used for subsequent experiments.
[0106] Friction performance test results are as follows Figure 4 As shown: The DPU-CD+AD-HA group has the lowest friction coefficient compared to other groups. Over time, it remains stable at a friction coefficient of less than 0.3, while the friction coefficient of the PU group is greater than 0.5.
[0107] The above experimental results indicate that the self-lubricating and self-repairing polyurethane meniscus material constructed by the present invention has good repair function. In different proportions of dimethylglyoxime, DPU2-CD has better mechanical characteristics while having self-repair efficiency, and DPU-CD+AD-HA exhibits good self-lubricating function.
[0108] Experimental Example 2: In vitro investigation of the biocompatibility of self-lubricating and self-repairing polyurethane meniscus materials
[0109] This experimental example includes a common PU group, i.e., adding pure PU material; a DPU group, i.e., adding DPU-CD material; and a DPU@HA group, i.e., adding DPU-CD+AD-HA material; the above materials are all prepared according to the method of Example 1 or Comparative Example 1.
[0110] 1. Experimental Methods
[0111] After the optimal ratio of the above-mentioned materials was screened out, chondrocytes were used as seed cells and loaded onto different polyurethane materials: the well plate group was used as a control, and the CCK-8 method and EDU method were used to detect the proliferation of cells on the scaffold material after three-dimensional co-culture; the activity of cells on the scaffold was observed using a laser confocal microscope after labeling with live and dead cell dyes; rhodamine-labeled phalloidin was used for cytoskeleton staining, the morphology of cells on the scaffold was observed, immunofluorescence was used to detect cartilage synthesis and catabolism, and migration and scratch experiments were used to detect cell migration ability.
[0112] 2. Experimental Results
[0113] After the chondrocyte co-culture experiment, we evaluated the cell viability of the different material groups by live-dead staining. Figure 5 As shown in a, 5f, on the 1st, 3rd and 7th days of co-culture, the number of living cells in the PU group, DPU group or DPU@HA group did not show statistically significant differences compared with the control group. This finding indicates that none of the three materials tested produced obvious cytotoxicity to chondrocytes. Further, in order to evaluate the effects of these materials on chondrocyte proliferation, we used EDU (5-ethynyl-2'-deoxyuridine) labeling and CCK-8 (cell counting kit-8) assays. The experimental results showed that there was no significant statistical difference in the cell proliferation levels of the PU group, DPU group and DPU@HA group compared with the control group ( Figure 5 b, 5e, 5g). This indicates that these materials have no inhibitory effect on the DNA proliferation of chondrocytes. Regarding cell migration ability, Figure 5c and 5d show that the three groups of materials did not show significant differences compared with the control group. In addition, we also evaluated the effects of the materials on the expression of chondrocyte synthesis and decomposition proteins by immunofluorescence technology. The results showed that there was no significant difference in the expression of the anabolic protein COL-2 (type II collagen) between the three groups of materials and the control group (see Figure 6 Similarly, no significant differences were observed in the expression of the catabolic protein MMP-13 (matrix metalloproteinase-13) (see Figure 6 b, 6c).
[0114] The above results indicate that these materials exhibit good biocompatibility with chondrocytes, neither inhibiting cell proliferation nor affecting cell migration ability, and have no negative impact on the synthesis and decomposition processes of chondrocytes.
[0115] Experimental Example 3: In vivo investigation of the effect of self-lubricating and self-repairing polyurethane meniscus prosthesis
[0116] This experimental example includes a PU group, i.e., adding pure PU material; and a DPU@HA group, i.e., adding DPU-CD+AD-HA material; the above materials are all prepared according to the method of Example 1 or Comparative Example 1.
[0117] 1. Experimental Methods
[0118] Male rabbits weighing 2.5-3.0 kg were selected for 6 and 12 weeks of experiments, and all rabbits were randomly divided into 3 groups: subtotal resection group (n=5 at each time point), PU material implantation group (n=5 at each time point), and DPU@HA implantation group (n=5 at each time point). In the implantation group, a rabbit medial meniscus resection model was first constructed, and the meniscus scaffolds of the PU or DPU@HA group were implanted to evaluate their in vivo applicability. The above meniscus scaffolds were soaked in 75% alcohol for 30 minutes and sterilized by ultraviolet light for 1 hour. All surgeries were performed under sterile conditions. Before surgery, sodium pentobarbital (3.5 mL / kg) was injected through the ear vein for anesthesia, fixed on the operating table, and the skin of the lower limbs on both sides was prepared and disinfected with iodine. Peel off the skin and subcutaneous tissue to expose the medial collateral ligament; cut the medial collateral ligament, open the joint capsule, and expose the medial meniscus; cut the connection between the posterior horn / anterior horn of the medial meniscus and the tibial plateau, and completely remove the medial meniscus; suture the polyurethane meniscus prosthesis constructed in the example to the ligament and joint capsule and fix it to the tibial plateau; close the joint cavity, and reconnect or suture the medial collateral ligament and other anatomical tissues with non-absorbable sutures, and then disinfect the leg with alcohol cotton balls; finally, return the rabbit to the cage to ensure its free movement, and inject penicillin intramuscularly once a day for 3 days after surgery to prevent infection. At 6 and 12 weeks after surgery, all rabbits were euthanized, and their femurs, tibias, and meniscus implants were removed for gross observation and histological evaluation. Figure 7 Shown is the placed polyurethane meniscus prosthesis (indicated by the yellow arrow and green dashed box).
[0119] Femtosecond laser multimodal scanning: The tibial plateau cartilage was cut into 2 mm slices with a blade, placed on the stage, and immediately tested on the machine. The wavelength was set to 900-1200 nm, the pulse frequency was 10 Hz, the pulse width was 5 fs, and the channels were set to two-photon fluorescence 2PFE, three-photon 3PFE, second harmonic SHG, and third harmonic THG.
[0120] 2. Experimental Results
[0121] like Figure 8 As shown in Figure 2, at 6 and 12 weeks after surgery, the articular cartilage of the femoral condyle, femoral trochlea, and tibial plateau of the three groups of rabbits were evaluated by gross observation and Micro CT scanning to quantitatively and qualitatively analyze the protective effect of cartilage. Figure 8As shown in a, 8b, 8c, and 8f: Through gross observation of the articular cartilage of the femoral condyle, femoral trochlea, and tibial plateau, the subtotal meniscectomy control group showed obvious cartilage degeneration, including severe wear of the tibial plateau and femoral condyle cartilage, and cartilage damage in the femoral trochlea area. MicroCT scan evaluation results showed that significant proliferation of osteophytes and significant collapse of the medial compartment were observed, accompanied by sclerosis of the subchondral bone. The degree of cartilage wear in the PU group ranged from moderate to severe. Although the meniscus function was restored to a certain extent, the cartilage protection effect was limited. The degree of cartilage wear in the DPU@HA group was mild, no osteophyte proliferation was observed, the medial compartment remained stable, and no sclerosis of the subchondral bone was observed ( Figure 8 d,8e,8g,8h).
[0122] like Fig. 9 As shown in the subtotal resection group, most of the cartilage collagen fibers were disordered, some were missing, and the metabolism was unbalanced ( Fig. 9 a), some fibers in the PU group are arranged in disorder and the structure is not complete ( Fig. 9 b), DPU@HA group has a similar structure to natural articular cartilage and is metabolically stable ( Fig. 9 c, 9d). The above results indicate that the self-lubricating and self-repairing polyurethane meniscus prosthesis has a cartilage-protective effect.
[0123] The above experimental examples prove that the self-lubricating and self-repairing polyurethane meniscus prosthesis constructed by the present invention not only has high modulus, high elasticity, and high lubrication properties, but also exhibits good biocompatibility and cartilage protection, and achieves the imitation of the dynamic self-repair and physiological cyclic lubrication of the natural meniscus, and has great potential application value in constructing meniscus substitutes.
Claims
1. A functionalized polyurethane, characterized in that: The invention comprises a self-repairing polyurethane elastomer and an adamantane-hyaluronic acid complex, wherein the adamantane-hyaluronic acid complex is covered on the surface of the self-repairing polyurethane elastomer, and the thickness of the adamantane-hyaluronic acid complex is 10-20 microns; The self-repairing polyurethane elastomer is made of the following raw materials in parts by weight: 1-2 parts of hard segment raw materials, Soft segment raw material 4.5-9 parts, 0.262-0.522 parts of dimethylglyoxime, Chain extender 0.412-0.824 parts, Cross-linking agent 0.04-0.08 parts; The adamantane-hyaluronic acid complex is made of the following raw materials in parts by weight: 10-20 parts of hyaluronic acid, 2.3-4.6 parts of diepoxide, Adamantane 0.5-5 parts.
2. The functionalized polyurethane according to claim 1, characterized in that The self-repairing polyurethane elastomer is made of the following raw materials in parts by weight: 1 part of hard segment raw material, 4.5 parts of soft segment raw material, 0.262-0.522 parts of dimethylglyoxime, Chain extender 0.412 parts, Crosslinking agent 0.04 parts.
3. The functionalized polyurethane according to claim 1, characterized in that: The self-repairing polyurethane elastomer is made of the following raw materials in parts by weight: 1 part of hard segment raw material, 4.5 parts of soft segment raw material, 0.392 parts of dimethylglyoxime, Chain extender 0.412 parts, Crosslinking agent 0.04 parts.
4. The functionalized polyurethane according to any one of claims 1 to 3, characterized in that: The adamantane-hyaluronic acid complex is made of the following raw materials in parts by weight: Hyaluronic acid 10 parts, 2.3 parts of diepoxide, Adamantane 0.5-5 parts.
5. The functionalized polyurethane according to claim 4, characterized in that: The adamantane-hyaluronic acid complex is made of the following raw materials in parts by weight: Hyaluronic acid 10 parts, 2.3 parts of diepoxide, Adamantane 5 parts.
6. The functionalized polyurethane according to claim 1, characterized in that: The hard segment raw material is selected from at least one of isophorone diisocyanate and polycaprolactone triol; And / or, the soft segment raw material is selected from at least one of polytetramethylene ether and polypropylene oxide; And / or, the chain extender is selected from at least one of 1,4-butanediol and glycerol; And / or, the cross-linking agent is selected from at least one of aminocyclodextrin and ethylenediamine; And / or, the diepoxy compound is selected from at least one of 1,4-butanediol diglycidyl ether and 1,6-hexanediol diglycidyl ether.
7. The method for preparing the functionalized polyurethane according to any one of claims 1 to 6, comprising the steps of: Step 1, reacting a hard segment raw material and a soft segment raw material to obtain a mixture A; Step 2, reacting mixture A with dimethylglyoxime to obtain mixture B; Step 3, reacting the mixture B with a chain extender and a crosslinker, and obtaining a self-repairing polyurethane elastomer after purification; Step 4, reacting hyaluronic acid with a diepoxide compound to obtain a mixture C; Step 5, reacting the mixture C with adamantane to obtain an adamantane-hyaluronic acid complex; Step 6, uniformly covering the surface of the self-repairing polyurethane elastomer with the adamantane-hyaluronic acid complex to obtain a self-lubricating-self-repairing polyurethane elastomer material.
8. The preparation method according to claim 7, characterized in that: In step 1, the reaction temperature is 60-80°C and the reaction time is 45 min-1.5 h; And / or, in step 2, the reaction temperature is 60-80°C and the reaction time is 1-2 h; and / or, in step 3, the reaction temperature is 60-80°C and the reaction time is 0.5-2 h; and / or, in step 4, the reaction temperature is 20-50°C and the reaction time is 6-12 h; And / or, in step 5, the reaction temperature is 40-80° C., and the reaction time is 12-36 h.
9. Use of the functionalized polyurethane according to any one of claims 1 to 6 in the preparation of a meniscus prosthesis.
10. A meniscus prosthesis, characterized in that: It is made of the functionalized polyurethane described in any one of claims 1 to 6.
Citation Information
Patent Citations
Shear force-responsive supramolecular bionic articular cartilage material with dynamic lubrication and self-repairing ability and preparation method thereof
CN110180022A
Disulfide bond-based bio-based degradable cross-linked self-repairing polyurethane and preparation method thereof
CN112126036A