Method for preparing high-purity vanadium pentoxide from high-concentration vanadium-containing solution
By hydrolyzing precipitated vanadium and washing ammonium-containing solutions in high-concentration vanadium solutions, the problems of low purity of vanadium products and wastewater are solved, the preparation of high-purity vanadium pentoxide and wastewater recycling are achieved, and the vanadium production efficiency and environmental protection are improved.
Patent Information
- Application Number
- CN202410901307.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-09-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The process of precipitating vanadium with acidic ammonium salts in high-concentration vanadium solutions results in low purity of vanadium products and the generation of a large amount of ammonia nitrogen wastewater. Although existing methods have been improved, they still have efficiency and wastewater problems.
By adding sulfuric acid to a high-concentration vanadium-containing solution to hydrolyze and precipitate vanadium, adjust the pH value to form sodium-containing polyvanadate, then use ammonium-containing solution to wash to remove sodium impurities, and finally calcine to obtain high-purity vanadium pentoxide. Recycling of washing liquid.
It significantly improves the purity of vanadium products, reduces ammonium salt consumption, and realizes the separation of ammonia nitrogen wastewater and the recovery of sodium salt, achieving efficient and clean vanadium production.
Smart Images

Figure CN118702145A
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-purity vanadium pentoxide preparation, and particularly relates to a method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution. Background Art
[0002] Vanadium is a strategic metal with important uses and is known as the "MSG of modern industry." In addition to its application in some traditional fields such as materials and chemicals, vanadium has also been used more in high-tech fields such as energy storage in recent years. Roasting-leaching is an important link in the extraction of vanadium from vanadium-containing minerals. The current mainstream roasting and leaching processes are sodium roasting-water leaching and calcium roasting-acid leaching. There are many vanadium-containing minerals and vanadium extraction methods, but no matter what raw materials and vanadium extraction methods are used, vanadium precipitation is required to precipitate vanadium from the solution through a vanadium precipitation process to obtain the final vanadium product. The main precipitants used in traditional vanadium precipitation methods are ammonium salts, iron salts and calcium salts. Acidic ammonium salt vanadium precipitation has been widely used in industrial production due to its short production cycle and high product purity.
[0003] As the demand for vanadium continues to increase, vanadium production companies are in urgent need of improving production efficiency. The use of high-concentration vanadium solution precipitation has met this demand. However, the acidic ammonium salt precipitation process has shortcomings for high-concentration vanadium-containing solutions: (1) Due to the high vanadium concentration, it is easier to form impurities such as sodium vanadate during the acidic ammonium salt precipitation process. It also causes the nucleation rate to be too fast, and the crystals formed are of different sizes, which are easy to carry impurities into the precipitation, resulting in low purity of the vanadium product. (2) It is inevitable to produce a large amount of ammonia nitrogen wastewater.
[0004] In response to the problem of vanadium precipitation from high-concentration vanadium solution, Chinese patent document CN113025833A discloses a method for vanadium precipitation from high-concentration vanadium solution, firstly, the vanadium-containing solution is adjusted to weak acidity, then melamine is added and the solution is adjusted to strong acidity, and finally, it is reacted under heating conditions for a period of time, and a vanadium-containing precipitate is obtained after filtration, and the vanadium-containing precipitate is calcined to obtain 98-grade vanadium pentoxide. Although this method can obtain qualified vanadium products, the price of the vanadium precipitation agent is relatively high, and organic vanadium precipitation wastewater is generated. Chinese patent document CN115676886A also discloses a method for vanadium precipitation from high-concentration vanadium solution, which firstly adjusts the solution to weak acidity, then mixes ammonium sulfate and vanadium precipitation wastewater and adds them to the high vanadium solution, and adjusts the pH to 2~2.1, and filters after boiling reaction to obtain the vanadium precipitation product. This method is essentially still vanadium precipitation with acidic ammonium salt of high-concentration vanadium solution, and the purity of the obtained vanadium product is still relatively low.
[0005] In summary, in order to improve the production efficiency of vanadium, the problem of vanadium precipitation in high-concentration vanadium solution still needs further research. Summary of the invention
[0006] In order to solve the problems of low product purity and large amount of ammonia nitrogen wastewater discharge in the process of acidic ammonium salt precipitation of vanadium in high-concentration vanadium solution, the present invention proposes a method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution. Compared with acidic ammonium salt precipitation of vanadium, the method not only reduces the consumption of ammonium salt, but also realizes the recycling of washing liquid under the premise of ensuring the purity of V2O5.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution comprises the following steps:
[0009] (1) adding sulfuric acid to a high-concentration vanadium-containing solution, adjusting the pH value of the vanadium-containing solution to be acidic to hydrolyze and precipitate vanadium, and obtaining sodium-containing polyvanadate after solid-liquid separation;
[0010] (2) washing the sodium-containing polyvanadate with an ammonium solution to remove sodium from the precipitate, and obtaining ammonium polyvanadate after solid-liquid separation;
[0011] (3) calcining the ammonium polyvanadate to obtain a high-purity vanadium pentoxide product.
[0012] Furthermore, the high-concentration vanadium-containing solution in step (1) refers to a solution obtained by sodium-roasting, water-leaching and impurity removal of vanadium-containing minerals or vanadium-containing slag.
[0013] Furthermore, the high-concentration vanadium-containing solution contains 40 to 80 g / L of vanadium, and the pH value is generally around 7, mainly containing vanadium and sodium elements. Usually, a vanadium concentration of ≥40 g / L is considered a high-concentration vanadium solution. Since the vanadium concentration is too high, the nucleation rate will be too fast, and the crystals formed will be of different sizes, which will easily carry impurities into the precipitation, and it will be more likely to form impurities such as sodium vanadate, resulting in a low purity of the vanadium product. Therefore, the existing acidic ammonium salt vanadium precipitation process is not suitable for high-concentration vanadium solutions.
[0014] Furthermore, the hydrolysis and precipitation of vanadium in step (1) refers to adding sulfuric acid to the high-concentration vanadium-containing solution to adjust the pH of the solution to 0.8-1.3.
[0015] During the acid hydrolysis and vanadium precipitation process of high-concentration vanadium-containing solution, if no heating is performed, the main existing form of vanadium at room temperature will change as follows: V 10 O 28 6‒ →HV 10 O 28 5‒ →H2V 10 O 28 4‒ →VO2 + Ultimately, vanadium exists mainly in the form of ions and cannot form precipitation.
[0016] Furthermore, in step (1), the reaction temperature for hydrolysis precipitation of vanadium is 95-100°C, and the reaction time is 20-50 min. The main reactions of vanadium during hydrolysis precipitation are as follows:
[0017] 6Na4H2V 10 O 28 + 7H2SO4 → 10NaHV6O 16 ↓ + 7Na2SO4 + 8H2O
[0018] 6(VO2)2SO4 + Na2SO4 + 7H2O → Na2V 12 O 31 ↓ + 7H2SO4
[0019] It can be seen that under heating conditions, all vanadium is converted into precipitation, avoiding the loss of vanadium. The applicant has found that when the pH of the hydrolysis vanadium precipitation is around 1 and the temperature is greater than 90°C, the precipitation rate of vanadium can reach more than 98%.
[0020] Furthermore, the solute in the ammonium-containing solution in step (2) is at least one of ammonium sulfate, ammonium carbonate, and ammonium bicarbonate. + The mass is 3 to 7 times the mass of sodium in the precipitate. + If the amount added is too large, the ammonia nitrogen wastewater content in the solution will be too high; if the amount added is too small, the sodium in the precipitate cannot be completely removed by washing.
[0021] Furthermore, in the washing and purification process in step (2), the ratio of the volume of the ammonium-containing solution (mL) to the sodium-containing polyvanadate precipitate (g) is 10-20:1, the washing temperature is 25-100°C, and the washing time is 15-30 min.
[0022] The main reactions that occur during the washing process are as follows:
[0023] NaHV6O 16 + 2NH4 + → (NH4)2V6O 16 + Na + + H +
[0024] Na2V 12 O 31 + 2NH4 + → (NH4)2V6O 16 + 2Na +
[0025] It should be noted that when using ammonium-containing solution to wash polyvanadates whose main impurity is sodium, NH4 + Not only can it replace the Na + , and further replaces H + , and H + The degree of substitution increases with the increase of washing temperature, NH4 + For H + The replacement of vanadium pentoxide does not affect the purity of the final vanadium pentoxide product. After washing, the washing liquid still mainly contains H + and NH4 + , can be returned to step (2) and continue to be used as washing water.
[0026] Furthermore, in step (3), the calcination temperature is 550-600°C, and the calcination time is 120-150 min.
[0027] The present invention also provides a high-purity vanadium pentoxide product prepared by the method, the purity of which is greater than 99.5%.
[0028] Compared with the mainstream vanadium precipitation process in industry, the technical solution of the present invention has the following advantages:
[0029] In this method, a high-concentration vanadium-containing solution (vanadium concentration greater than 40 g / L) is first subjected to acid hydrolysis to precipitate vanadium. In this process, sodium ions combine with vanadate ions to enter the precipitate, and after solid-liquid separation, a polyvanadate precipitate with sodium as the main impurity is obtained. Then, according to NH4 + The ability to bind to vanadate is greater than that of Na + The polyvanadate precipitate is washed and purified with an ammonium solution to convert the sodium-containing polyvanadate into ammonium polyvanadate, thereby achieving the purpose of purification; the ammonium polyvanadate after solid-liquid separation is calcined to obtain a high-purity vanadium pentoxide product, and the washing liquid is returned to the washing and purification process.
[0030] By using the present invention to treat high-concentration vanadium-containing solutions, not only can the amount of ammonium salt used be reduced compared to the traditional ammonium salt vanadium precipitation method, but the washing liquid can also be recycled. In addition, the separation of high-concentration sodium salt and ammonia nitrogen wastewater in vanadium precipitation wastewater is achieved, providing a basis for recovering a large amount of high-purity sodium salt in wastewater, and realizing clean and efficient production of vanadium. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Some drawings involved in the embodiments are briefly described to more effectively describe the relevant embodiments of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1This is a phase analysis diagram of the hydrolysis vanadium precipitation product in Example 1 of the present invention;
[0033] Figure 2 This is a SEM-EDS analysis diagram of the washed product in Example 1 of the present invention;
[0034] Figure 3 This is a phase analysis diagram of the calcined product in Example 1 of the present invention;
[0035] Figure 4 The following is the phase analysis and physical picture of the washed product in Example 2 of the present invention. DETAILED DESCRIPTION
[0036] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0037] Example 1
[0038] The solution of vanadium-containing converter slag after sodium roasting, water leaching and impurity removal was used as the raw material. The solution mainly contained vanadium and sodium elements, with a pH of 7, a vanadium concentration of 40 g / L, and a sodium concentration of 39 g / L. 100 mL of vanadium solution was placed in a beaker, and the pH of the vanadium solution was adjusted to 1 with sulfuric acid. The beaker was placed in a heat-collecting magnetic stirrer and kept warm at 100 °C for 40 min, with the magnetic speed maintained at 400 rpm. After the hydrolysis and precipitation of vanadium, a vacuum filter was used for solid-liquid separation to obtain a sodium-containing polyvanadate precipitate. According to the ratio of ammonium sulfate solution volume (mL) to sodium-containing polyvanadate precipitate (g) of 20:1, the sodium-containing polyvanadate and NH4 + An ammonium sulfate solution with a mass 5 times that of the sodium in the precipitate was mixed in a beaker and stirred at 25 °C for 20 min. The stirring speed was set to 500 rpm. After the reaction, a washing product was obtained by solid-liquid separation. The washing product was calcined in a muffle furnace at 550 °C for 120 min to obtain high-purity vanadium pentoxide.
[0039] Figure 1 This is the XRD diagram of the hydrolysis vanadium precipitation product, indicating that the phase of the hydrolysis vanadium precipitation product is mainly sodium vanadate. Figure 2 This is the SEM-EDS analysis diagram of the washed product, which shows that after washing with an ammonium solution, the distribution of vanadium and oxygen in the washed product is consistent, and sodium is basically removed. Figure 3 The figure is a phase analysis diagram of the calcined product, indicating that the main phase of the calcined product is vanadium pentoxide. The purity of vanadium pentoxide is shown in Table 1.
[0040] Example 2
[0041] The solution of vanadium-containing converter slag after sodium roasting, water leaching and impurity removal is used as the raw material. The solution mainly contains vanadium and sodium elements, with a pH of 7, of which the concentration of vanadium is 40 g / L and the concentration of sodium is 39 g / L. The concentration of vanadium in the solution is 40 g / L. 100mL of vanadium solution was placed in a beaker, and the pH of the vanadium solution was adjusted to 1 with sulfuric acid. The beaker was placed in a heat-collecting magnetic stirrer and kept warm at 100 °C for 40 min, with a stirring speed of 400 rpm. After the hydrolysis and precipitation of vanadium, a vacuum filter was used for solid-liquid separation to obtain a sodium-containing polyvanadate precipitate. According to the ratio of ammonium sulfate solution volume (mL) to sodium-containing polyvanadate precipitate (g) of 20:1, the sodium-containing polyvanadate and NH4 + An ammonium sulfate solution with a mass four times that of the sodium in the precipitate was mixed in a beaker and stirred at 100 °C for 20 min. The stirring speed was set to 500 rpm. After the reaction, a washing product was obtained by solid-liquid separation. The washing product was calcined in a muffle furnace at 550 °C for 120 min to obtain high-purity vanadium pentoxide.
[0042] Figure 4 The phase analysis and physical picture of the washed product in Example 2 illustrate that the sodium-containing polyvanadate is converted into ammonium polyvanadate after being washed with ammonium sulfate at 100°C. The purity of vanadium pentoxide is shown in Table 1.
[0043] Example 3
[0044] The solution of vanadium-containing converter slag after sodium roasting, water leaching and impurity removal is used as raw material. The solution mainly contains vanadium and sodium elements, with a pH of 7.2, of which the concentration of vanadium is 80 g / L and the concentration of sodium is 83 g / L. The concentration of vanadium in the solution is 80 g / L. 100mL of vanadium solution was placed in a beaker, and the pH of the vanadium solution was adjusted to 1 with sulfuric acid. The beaker was placed in a heat-collecting magnetic stirrer and kept warm at 100 °C for 30 min, with the magnetic speed maintained at 400 rpm. After the hydrolysis and precipitation of vanadium, a vacuum filter was used for solid-liquid separation. According to the ratio of ammonium sulfate solution volume (mL) to sodium-containing polyvanadate precipitate (g) of 20:1, the sodium-containing polyvanadate and NH4 + An ammonium sulfate solution with a mass 7 times that of the sodium in the precipitate was mixed in a beaker and stirred at 25 °C for 30 min. The stirring speed was set to 500 rpm. After the reaction was completed, the solid-liquid separation was performed and the washed product was calcined in a muffle furnace at 600 °C for 120 min to obtain high-purity vanadium pentoxide. The purity of vanadium pentoxide is shown in Table 1.
[0045] Example 4
[0046] The solution of vanadium-containing stone coal after sodium roasting, water leaching and impurity removal was used as the raw material. The solution mainly contained vanadium and sodium elements, with a pH of 7, of which the concentration of vanadium was 40 g / L and the concentration of sodium was 41 g / L. 100 mL of vanadium solution was placed in a beaker, and the pH of the vanadium solution was adjusted to 1.3 with sulfuric acid. The beaker was placed in a stirrer and kept warm at 100 °C for 40 min, with a speed of 400 rpm. After the hydrolysis and precipitation of vanadium, a vacuum filter was used for solid-liquid separation. According to the ratio of ammonium sulfate solution volume (mL) to sodium polyvanadate precipitate (g) of 10:1, the sodium polyvanadate and NH4 + An ammonium sulfate solution with a mass three times that of the sodium in the precipitate was mixed in a beaker and stirred at 25 °C for 30 min. The stirring speed was set to 500 rpm. After the reaction was completed, the solid-liquid separation was performed and the washed product was calcined in a muffle furnace at 600 °C for 120 min to obtain high-purity vanadium pentoxide. The purity of vanadium pentoxide is shown in Table 1.
[0047] Comparative Example 1
[0048] According to the ratio of ammonium sulfate solution volume (mL) to sodium polyvanadate precipitate (g) of 20:1, the sodium polyvanadate obtained in Example 1 was mixed with NH4 + An ammonium sulfate solution with a mass twice that of the sodium in the precipitate was mixed in a beaker, stirred at 25°C for 20 min, and the stirring speed was set to 500 rpm. After the reaction, a washing product was obtained by solid-liquid separation, and the washing product was calcined in a muffle furnace at 550°C for 120 min to obtain high-purity vanadium pentoxide, the purity of which is shown in Table 1. It can be seen that when the concentration of the ammonium sulfate solution is low, the purity of the obtained vanadium pentoxide is very low.
[0049] Comparative Example 2
[0050] According to the ratio of ammonium sulfate solution volume (mL) to sodium polyvanadate precipitate (g) of 25:1, the sodium polyvanadate obtained in Example 1 was mixed with NH4 + An ammonium sulfate solution with a mass 5 times that of the sodium in the precipitate was mixed in a beaker, stirred and reacted at 25 °C for 20 min, and the stirring speed was set to 500 rpm. After the reaction, a washing product was obtained by solid-liquid separation, and the washing product was calcined in a muffle furnace at 550 °C for 120 min to obtain high-purity vanadium pentoxide, the purity of which is shown in Table 1. It can be seen that when the ratio of the volume of ammonium sulfate solution (mL) to the sodium-containing polyvanadate precipitate (g) exceeds 20, the purity of the obtained vanadium pentoxide is low.
[0051] Comparative Example 3
[0052] According to the ratio of ammonium sulfate solution volume (mL) to sodium polyvanadate precipitate (g) of 5:1, the sodium polyvanadate obtained in Example 1 was mixed with NH4 +An ammonium sulfate solution with a mass 5 times that of the sodium in the precipitate was mixed in a beaker, stirred and reacted at 25 °C for 20 min, and the stirring speed was set to 500 rpm. After the reaction, a washing product was obtained by solid-liquid separation, and the washing product was calcined in a muffle furnace at 550 °C for 120 min to obtain high-purity vanadium pentoxide, the purity of which is shown in Table 1. It can be seen that when the ratio of the volume of ammonium sulfate solution (mL) to the sodium-containing polyvanadate precipitate (g) is less than 10, the purity of the obtained vanadium pentoxide is also low.
[0053] Comparative Example 4
[0054] Using the vanadium-containing solution in Example 1 as a raw material, 100 mL of vanadium solution was placed in a beaker, and conventional acidic ammonium salt was used to precipitate vanadium. Ammonium sulfate was added according to an ammonium addition coefficient of 1.2, and the pH of the vanadium solution was adjusted to 2 with sulfuric acid, and the mixture was kept at 100 °C for 40 min, and the magnetic speed was maintained at 400 rpm. After the reaction was completed, polyammonium vanadate was obtained by solid-liquid separation, and the polyammonium vanadate was calcined in a muffle furnace at 550 °C for 120 min to obtain vanadium pentoxide, and the purity was shown in Table 1.
[0055] Comparative Example 5
[0056] Using the vanadium-containing solution in Example 1 as a raw material, 100 mL of the vanadium solution was placed in a beaker, the pH of the vanadium solution was adjusted to 1 with sulfuric acid, and the beaker was placed in a heat-collecting magnetic stirrer, kept at 25°C for 40 min, and the magnetic speed was maintained at 400 rpm. The precipitation rate of vanadium was only 10.5%.
[0057] Table 1 Purity and yield of vanadium pentoxide in the examples and comparative examples
[0058]
[0059] The purity of V2O5 in the examples in Table 1 is above 99.5%, which meets the industrial requirement for high-purity vanadium pentoxide with a purity greater than 99.5%. The purity of the comparative examples is lower, which does not meet the industrial requirement for high-purity vanadium pentoxide.
[0060] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution, characterized in that: The following steps are involved: (1) adding sulfuric acid to a high-concentration vanadium-containing solution, adjusting the pH value of the vanadium-containing solution to be acidic to hydrolyze and precipitate vanadium, and obtaining sodium-containing polyvanadate after solid-liquid separation; (2) washing the sodium-containing polyvanadate with an ammonium-containing solution to obtain ammonium polyvanadate after solid-liquid separation; (3) calcining the ammonium polyvanadate to obtain a high-purity vanadium pentoxide product.
2. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 1, characterized in that: The high-concentration vanadium-containing solution in step (1) refers to a solution obtained by sodium roasting, water leaching and impurity removal of vanadium-containing minerals or vanadium-containing slag, wherein the vanadium content is 40-80 g / L.
3. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 2, characterized in that: The hydrolysis precipitation of vanadium in step (1) is to add sulfuric acid to the high concentration vanadium-containing solution to adjust the pH of the solution to 0.8-1.
3.
4. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 3, characterized in that: In step (1), the reaction temperature for hydrolysis and precipitation of vanadium is 95-100°C, and the reaction time is 20-50 min.
5. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 1, characterized in that: The solute in the ammonium-containing solution in step (2) is at least one of ammonium sulfate, ammonium carbonate and ammonium bicarbonate.
6. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 5, characterized in that: NH4 in the ammonium solution used in step (2) + The mass is 3 to 7 times the mass of sodium in the precipitate.
7. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 6, characterized in that: In the washing and purification process described in step (2), the ratio of the volume (mL) of the ammonium-containing solution to the volume (g) of the sodium-containing polyvanadate precipitate is 10-20:1, the washing temperature is 25-100°C, and the washing time is 15-30 min.
8. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 7, characterized in that: The washing liquid after washing in step (2) is continued to be used as washing water.
9. The method for preparing high-purity vanadium pentoxide from a high-concentration vanadium-containing solution according to claim 1, characterized in that: In step (3), the calcination temperature is 550-600°C and the calcination time is 120-150 min.
10. The high-purity vanadium pentoxide product prepared by the method according to any one of claims 1 to 9, characterized in that: The purity of the high-purity vanadium pentoxide product is greater than 99.5%.
Citation Information
Patent Citations
Method for precipitating vanadium from high-concentration vanadium liquid
CN113025833A
Vanadium precipitation method for reducing vanadium precipitation wastewater of high-concentration vanadium liquid
CN115676886A
Process for producing vanadium pentoxide by vanadium-contained solution
CN102336437A
Production technology of harmless high-purity vanadium pentoxide
CN103145187A
Hydrochloric acid vanadium precipitation method for sodium salt roasting water leaching purification liquid
CN113151684A
Cited By
Method for preparing vanadium pentoxide by using vanadium-rich liquid with relatively high impurity content
CN119551721A
A method for preparing vanadium pentoxide from a vanadium-rich solution having a high content of impurities
CN119551721B