Anti-slip and anti-fouling tile and production process thereof
The composite material is prepared by modifying filler and silicon carbide ball mill, combined with ultrasonic treatment and impregnation and lifting process, a composite sol and long-chain fluorane film is formed, which solves the problem of poor anti-slip and anti-fouling effect of ceramic tiles and achieves significant anti-slip and anti-fouling and anti-fouling Performance improvement.
Patent Information
- Application Number
- CN202411194948.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-29
AI Technical Summary
At this stage, the anti-slip and anti-fouling effect of ceramic tiles is poor, easy to be contaminated and have a high water absorption rate, making it difficult to remove stains. The anti-slip effect is reduced when water stains are used after the anti-slip agent is used, which increases safety risks.
The composite material is prepared by modified filler and silicon carbide ball mill, and the silica sol is formed by hydrolysis and condensation of ethyl orthosilicate. Combined with ultrasonic treatment and impregnation and lifting process, the composite sol is formed and in a heptadecafluorodecyl trimethoxysilane solution. Treatment to form a long-chain fluorane film to reduce stain adsorption, and ion exchange is used for epoxy cyclodextrin and lithium ions to reduce contaminant adhesion.
The anti-slip and anti-fouling properties of ceramic tiles are significantly improved, and the surface roughness is increased by forming small holes and the long-chain fluorane film is reduced in stain adsorption. It also contains titanium dioxide structure to catalyze the decomposition of organic matter and reduce stain adhesion.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tile preparation, and in particular to an anti-slip and anti-fouling tile and a production process thereof. Background Art
[0002] Ceramic tiles are a kind of acid- and alkali-resistant porcelain or stone material made of refractory metal oxides and semi-metal oxides through grinding, mixing, pressing, glazing, and sintering. They are used as building or decorative materials. The raw materials are mostly made of a mixture of clay, quartz sand, etc. According to the use, they are divided into: exterior wall tiles, interior wall tiles, floor tiles, square tiles, industrial tiles, etc. According to the production process, they are divided into: printed tiles, polished tiles, spotted tiles, crystal tiles, and unglazed tiles. In daily use, ceramic tiles are often contaminated by pollutants such as ink, paint, tea, and oil, leaving difficult-to-remove stains on their surfaces. Generally, the greater the water absorption rate of ceramic tiles, the greater the degree of susceptibility to pollution. At present, in order to further improve the anti-fouling ability of ceramic tiles, most polished tile manufacturers use anti-fouling agents during production to make up for the poor anti-fouling performance of the polished tile surface due to production process reasons. At the same time, when water stains appear on the surface, the anti-slip effect is greatly reduced, thereby increasing the risk factor. Summary of the invention
[0003] The purpose of the present invention is to provide a non-slip and non-fouling ceramic tile and a production process thereof, so as to solve the problem that the non-slip and non-fouling effects of ceramic tiles at present are poor.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A production process for anti-slip and anti-fouling tiles, specifically comprising the following steps:
[0006] Step A1: The modified filler, silicon carbide and deionized water are mixed and ball-milled to obtain a composite material, the composite material, tetraethyl orthosilicate and ethanol are mixed, stirred at a speed of 200-300 r / min and a temperature of 20-25° C., and ammonia water and deionized water are added to react for 4-6 hours, and then aged at a temperature of 40-50° C. for 10-15 hours to obtain a composite sol;
[0007] Step A2: soaking the tile substrate in deionized water, ultrasonically treating it for 20-30 minutes at a frequency of 30-40 kHz, taking it out and soaking it in acetone, ultrasonically treating it for 30-40 minutes, taking it out and soaking it in ethanol, ultrasonically treating it for 30-40 minutes, taking it out and drying it to obtain a pretreated substrate;
[0008] Step A3: Immerse the pretreated substrate in the composite sol, immerse and pull it at a speed of 5 cm / min, and then dry it at a temperature of 80-90°C for 10-15 minutes. Repeat the immersion, pulling and drying for 3-5 times, and sinter it at a temperature of 1250-1300°C for 3-5 hours to obtain a modified substrate. Mix heptadecafluorodecyltrimethoxysilane and ethanol evenly, immerse the modified substrate therein, add deionized water, and ultrasonically treat it at a frequency of 20-30kHz for 15-20 minutes. Take it out and dry it to obtain anti-slip and anti-fouling tiles.
[0009] Furthermore, the mass ratio of the modified filler, silicon carbide and deionized water described in step A1 is 1:1:0.8, the usage ratio of the composite material, tetraethyl orthosilicate, ethanol, ammonia water and deionized water is 1g:5mL:15mL:10mL:8mL, and the concentration of ammonia water is 1mol / L.
[0010] Furthermore, the volume ratio of heptadecafluorodecyltrimethoxysilane, ethanol and deionized water in step A3 is 1:10:3.
[0011] Further, the modified filler is prepared by the following steps:
[0012] Step B1: mixing hexagonal boron nitride, sodium hydroxide and ethanol, reacting for 4-6 hours at a speed of 600-800 r / min and a temperature of 120-125° C. to obtain hydroxy boron nitride; mixing hydroxy boron nitride, isocyanatepropyltriethoxysilane and DMF, reacting for 3-5 hours at a speed of 120-150 r / min and a temperature of 20-25° C. to obtain modified boron nitride;
[0013] Step B2: β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and DMF are mixed evenly, reacted for 2-3 hours at a speed of 120-150 r / min and a temperature of 65-70° C., and then sodium hydroxide solution is added, the temperature is raised to 75-80° C., and the reaction is carried out for 3-5 hours to obtain epoxy cyclodextrin. Epoxy cyclodextrin, aspartic acid and DMF are mixed evenly, reacted for 4-6 hours at a speed of 200-300 r / min, a temperature of 30-40° C., and a pH value of 10-11, and the pH is adjusted to be acidic to obtain modified cyclodextrin;
[0014] Step B3: Mix the modified cyclodextrin, lithium hydroxide and DMF, stir for 1-1.5h at a speed of 300-500r / min and a temperature of 20-25°C to obtain a precursor, mix the modified boron nitride, tetraethyl orthosilicate, precursor, DMF and ethanol evenly, stir and add deionized water and hydrochloric acid at a speed of 120-150r / min and a temperature of 65-70°C, react for 2-3h, add tetrabutyl titanate, continue to react for 3-4h, heat to 120-130°C, keep warm for 1-2h to obtain a modified filler.
[0015] Furthermore, the amount ratio of hexagonal boron nitride, sodium hydroxide and ethanol in step B1 is 1g:15g:80mL, and the amount ratio of hydroxyboron nitride and triethoxypropyl isocyanate is 1g:32mL.
[0016] Furthermore, the dosage ratio of β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution in step B2 is 3g:1g:0.5g:30mL, the mass fraction of the sodium hydroxide solution is 10%, and the molar ratio of the epoxy group on the epoxycyclodextrin to aspartic acid is 1:1.
[0017] Furthermore, the amount ratio of the modified cyclodextrin, lithium hydroxide and DMF described in step B3 is 1g:8g:20mL, the amount ratio of modified boron nitride, tetraethyl orthosilicate, precursor, deionized water, hydrochloric acid solution and tetrabutyl titanate is 1g:80mmol:3g:10mL:3mL:20mmol, and the mass fraction of the hydrochloric acid solution is 1.5%.
[0018] The beneficial effects of the present invention are as follows: the anti-skid and anti-fouling ceramic tile prepared by the present invention is prepared by ball-milling modified filler and silicon carbide as raw materials to obtain a composite material, the composite material is mixed with tetraethyl orthosilicate, and then under the action of ammonia water, the tetraethyl orthosilicate is hydrolyzed and condensed to form silica sol to obtain a composite sol, the surface of the ceramic tile substrate is cleaned to obtain a pretreated substrate, the pretreated substrate is immersed in the composite sol, dipped and pulled, dried and sintered, and finally immersed in a heptadecafluorodecyltrimethoxysilane solution to obtain the anti-skid and anti-fouling ceramic tile.
[0019] The modified filler is prepared by treating hexagonal boron nitride with sodium hydroxide to form hydroxyl boron nitride, reacting hydroxyl boron nitride with isocyanate propyl triethoxysilane so that the hydroxyl group on the hydroxyl boron nitride reacts with the isocyanate group on the isocyanate propyl triethoxysilane to obtain modified boron nitride, reacting β-cyclodextrin with epichlorohydrin so that the hydroxyl group on the β-cyclodextrin reacts with the epoxy group on the epichlorohydrin, and then forming a new epoxy group under the action of sodium hydroxide solution to obtain epoxy cyclodextrin, reacting epoxy cyclodextrin with aspartic acid so that the epoxy group on the epoxy cyclodextrin reacts with the amino group on the aspartic acid to obtain modified cyclodextrin, blending the modified cyclodextrin with lithium hydroxide so that the carboxyl group on the modified cyclodextrin is complexed with lithium ions and the cavity in the cyclodextrin is coated with lithium hydroxide to obtain a precursor, and hydrolyzing and polymerizing the modified boron nitride, ethyl orthosilicate, the precursor and tetrabutyl titanate to obtain the modified filler.
[0020] After the pre-treated substrate is immersed and pulled in the composite sol, a glaze will be formed on the surface during sintering. However, due to the presence of cyclodextrin, the cyclodextrin will be carbonized and fall off, causing tiny holes in the glaze on the surface. The presence of holes will increase the roughness of the tile surface, thereby increasing the anti-slip effect of the tile. Finally, it is immersed in a solution of heptadecafluorodecyltrimethoxysilane. Under the action of deionized water, the siloxane on the heptadecafluorodecyltrimethoxysilane will be hydrolyzed and grafted with the hydroxyl groups on the glaze surface, and enter the surface holes at the same time to form a long-chain fluorocarbon film, which can reduce the surface energy to avoid stain adsorption, and contains a titanium dioxide structure. When exposed to light, it can catalyze the decomposition of organic matter and reduce the possibility of stain adsorption. Under the action of electrostatic attraction, lithium ions can diffuse from the glaze to the hydration layer, adsorb on negatively charged oxygen ions, and come into contact with pollutants with hydroxyl groups to undergo ion exchange, turning the pollutants into hydrophilic substances, reducing the adhesion of pollutants to tiles, and achieving an anti-fouling effect. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Embodiment 1 A production process of anti-slip and anti-fouling tiles comprises the following steps:
[0023] Step A1: The modified filler, silicon carbide and deionized water are mixed and ball-milled to obtain a composite material, the composite material, tetraethyl orthosilicate and ethanol are mixed, stirred at a speed of 200 r / min and a temperature of 20° C., and ammonia water and deionized water are added to react for 4 hours, and then aged at a temperature of 40° C. for 10 hours to obtain a composite sol;
[0024] Step A2: soaking the tile substrate in deionized water, ultrasonically treating it for 20 minutes at a frequency of 30 kHz, taking it out and soaking it in acetone, ultrasonically treating it for 30 minutes, taking it out and soaking it in ethanol, ultrasonically treating it for 30 minutes, taking it out and drying it to obtain a pretreated substrate;
[0025] Step A3: Immerse the pretreated substrate in the composite sol, immerse and pull it at a speed of 5 cm / min, and then dry it at a temperature of 80°C for 10 minutes. Repeat the immersion, pulling and drying for 3 times, and sinter it at a temperature of 1250°C for 3 hours to obtain a modified substrate. Mix heptadecafluorodecyltrimethoxysilane and ethanol evenly, immerse the modified substrate therein, add deionized water, and ultrasonically treat it at a frequency of 20 kHz for 15 minutes. Take it out and dry it to obtain anti-slip and anti-fouling tiles.
[0026] The mass ratio of the modified filler, silicon carbide and deionized water described in step A1 is 1:1:0.8, the usage ratio of the composite material, tetraethyl orthosilicate, ethanol, ammonia water and deionized water is 1g:5mL:15mL:10mL:8mL, and the concentration of ammonia water is 1mol / L.
[0027] The volume ratio of heptadecafluorodecyltrimethoxysilane, ethanol and deionized water in step A3 is 1:10:3.
[0028] The modified filler is prepared by the following steps:
[0029] Step B1: Hexagonal boron nitride, sodium hydroxide and ethanol are mixed, and the mixture is reacted at a speed of 600 r / min and a temperature of 120° C. for 4 h to obtain hydroxy boron nitride; hydroxy boron nitride, isocyanatepropyltriethoxysilane and DMF are mixed, and the mixture is reacted at a speed of 120 r / min and a temperature of 20° C. for 3 h to obtain modified boron nitride;
[0030] Step B2: β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and DMF are mixed evenly, reacted at a speed of 120 r / min and a temperature of 65° C. for 2 h, and then a sodium hydroxide solution is added, the temperature is raised to 75° C., and the reaction is carried out for 3 h to obtain epoxy cyclodextrin; epoxy cyclodextrin, aspartic acid and DMF are mixed evenly, reacted at a speed of 200 r / min, a temperature of 30° C., and a pH value of 10 for 4 h, and the pH is adjusted to be acidic to obtain modified cyclodextrin;
[0031] Step B3: Mix the modified cyclodextrin, lithium hydroxide and DMF, stir for 1 hour at a speed of 300 r / min and a temperature of 20°C to obtain a precursor, mix the modified boron nitride, tetraethyl orthosilicate, precursor, DMF and ethanol evenly, stir and add deionized water and hydrochloric acid at a speed of 120 r / min and a temperature of 65°C, react for 2 hours, add tetrabutyl titanate, continue to react for 3 hours, heat to 120°C, and keep warm for 1 hour to obtain a modified filler.
[0032] The amount ratio of hexagonal boron nitride, sodium hydroxide and ethanol described in step B1 is 1g:15g:80mL, and the amount ratio of hydroxyboron nitride and triethoxypropyl isocyanate is 1g:32mL.
[0033] The amount ratio of β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution in step B2 is 3g:1g:0.5g:30mL, the mass fraction of the sodium hydroxide solution is 10%, and the molar ratio of the epoxy group on the epoxycyclodextrin to aspartic acid is 1:1.
[0034] The amount ratio of the modified cyclodextrin, lithium hydroxide and DMF described in step B3 is 1g:8g:20mL, the amount ratio of modified boron nitride, tetraethyl orthosilicate, precursor, deionized water, hydrochloric acid solution and tetrabutyl titanate is 1g:80mmol:3g:10mL:3mL:20mmol, and the mass fraction of the hydrochloric acid solution is 1.5%.
[0035] Embodiment 2 A production process of anti-slip and anti-fouling tiles comprises the following steps:
[0036] Step A1: The modified filler, silicon carbide and deionized water are mixed and ball-milled to obtain a composite material, the composite material, tetraethyl orthosilicate and ethanol are mixed, stirred at a speed of 200 r / min and a temperature of 25° C., and ammonia water and deionized water are added to react for 5 hours, and then aged at a temperature of 45° C. for 13 hours to obtain a composite sol;
[0037] Step A2: soaking the tile substrate in deionized water, ultrasonically treating it for 25 minutes at a frequency of 35 kHz, taking it out and soaking it in acetone, ultrasonically treating it for 35 minutes, taking it out and soaking it in ethanol, ultrasonically treating it for 3.5 minutes, taking it out and drying it to obtain a pretreated substrate;
[0038] Step A3: Immerse the pretreated substrate in the composite sol, immerse and pull it at a speed of 5 cm / min, and then dry it at a temperature of 85°C for 15 minutes. Repeat the immersion, pulling and drying for 4 times, and sinter it at a temperature of 1250°C for 4 hours to obtain a modified substrate. Mix heptadecafluorodecyltrimethoxysilane and ethanol evenly, soak the modified substrate therein, add deionized water, and ultrasonically treat it at a frequency of 25 kHz for 18 minutes. Take it out and dry it to obtain anti-slip and anti-fouling tiles.
[0039] The mass ratio of the modified filler, silicon carbide and deionized water described in step A1 is 1:1:0.8, the usage ratio of the composite material, tetraethyl orthosilicate, ethanol, ammonia water and deionized water is 1g:5mL:15mL:10mL:8mL, and the concentration of ammonia water is 1mol / L.
[0040] The volume ratio of heptadecafluorodecyltrimethoxysilane, ethanol and deionized water in step A3 is 1:10:3.
[0041] The modified filler is prepared by the following steps:
[0042] Step B1: Hexagonal boron nitride, sodium hydroxide and ethanol are mixed, and the mixture is reacted at a speed of 600 r / min and a temperature of 125° C. for 5 h to obtain hydroxy boron nitride; hydroxy boron nitride, isocyanatepropyltriethoxysilane and DMF are mixed, and the mixture is reacted at a speed of 120 r / min and a temperature of 23° C. for 4 h to obtain modified boron nitride;
[0043] Step B2: β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and DMF are mixed evenly, reacted at a speed of 120 r / min and a temperature of 68° C. for 2.5 hours, and then a sodium hydroxide solution is added, the temperature is raised to 78° C., and the reaction is carried out for 4 hours to obtain epoxy cyclodextrin. Epoxy cyclodextrin, aspartic acid and DMF are mixed evenly, reacted at a speed of 200 r / min, a temperature of 35° C., and a pH value of 11 for 5 hours, and the pH is adjusted to be acidic to obtain modified cyclodextrin;
[0044] Step B3: Mix the modified cyclodextrin, lithium hydroxide and DMF, stir for 1 hour at a speed of 300 r / min and a temperature of 25°C to obtain a precursor, mix the modified boron nitride, tetraethyl orthosilicate, precursor, DMF and ethanol evenly, stir and add deionized water and hydrochloric acid at a speed of 150 r / min and a temperature of 65°C, react for 2 hours, add tetrabutyl titanate, continue to react for 4 hours, heat to 125°C, and keep warm for 2 hours to obtain a modified filler.
[0045] The amount ratio of hexagonal boron nitride, sodium hydroxide and ethanol described in step B1 is 1g:15g:80mL, and the amount ratio of hydroxyboron nitride and triethoxypropyl isocyanate is 1g:32mL.
[0046] The amount ratio of β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution in step B2 is 3g:1g:0.5g:30mL, the mass fraction of the sodium hydroxide solution is 10%, and the molar ratio of the epoxy group on the epoxycyclodextrin to aspartic acid is 1:1.
[0047] The amount ratio of the modified cyclodextrin, lithium hydroxide and DMF described in step B3 is 1g:8g:20mL, the amount ratio of modified boron nitride, tetraethyl orthosilicate, precursor, deionized water, hydrochloric acid solution and tetrabutyl titanate is 1g:80mmol:3g:10mL:3mL:20mmol, and the mass fraction of the hydrochloric acid solution is 1.5%.
[0048] Embodiment 3 A production process of anti-slip and anti-fouling tiles comprises the following steps:
[0049] Step A1: The modified filler, silicon carbide and deionized water are mixed and ball-milled to obtain a composite material, the composite material, tetraethyl orthosilicate and ethanol are mixed, stirred at a speed of 300 r / min and a temperature of 25° C., and ammonia water and deionized water are added to react for 6 hours, and then aged at a temperature of 50° C. for 15 hours to obtain a composite sol;
[0050] Step A2: soaking the tile substrate in deionized water, ultrasonically treating it for 30 minutes at a frequency of 40 kHz, taking it out and soaking it in acetone, ultrasonically treating it for 40 minutes, taking it out and soaking it in ethanol, ultrasonically treating it for 40 minutes, taking it out and drying it to obtain a pretreated substrate;
[0051] Step A3: Immerse the pretreated substrate in the composite sol, immerse and pull it at a speed of 5 cm / min, and then dry it at a temperature of 90°C for 15 minutes. Repeat the immersion, pulling and drying for 5 times, and sinter it at a temperature of 1300°C for 5 hours to obtain a modified substrate. Mix heptadecafluorodecyltrimethoxysilane and ethanol evenly, immerse the modified substrate therein, add deionized water, and ultrasonically treat it at a frequency of 30 kHz for 20 minutes. Take it out and dry it to obtain anti-slip and anti-fouling tiles.
[0052] The mass ratio of the modified filler, silicon carbide and deionized water described in step A1 is 1:1:0.8, the usage ratio of the composite material, tetraethyl orthosilicate, ethanol, ammonia water and deionized water is 1g:5mL:15mL:10mL:8mL, and the concentration of ammonia water is 1mol / L.
[0053] The volume ratio of heptadecafluorodecyltrimethoxysilane, ethanol and deionized water in step A3 is 1:10:3.
[0054] The modified filler is prepared by the following steps:
[0055] Step B1: Hexagonal boron nitride, sodium hydroxide and ethanol are mixed, and the mixture is reacted at a speed of 800 r / min and a temperature of 125° C. for 6 hours to obtain hydroxy boron nitride; hydroxy boron nitride, isocyanatepropyltriethoxysilane and DMF are mixed, and the mixture is reacted at a speed of 150 r / min and a temperature of 25° C. for 5 hours to obtain modified boron nitride;
[0056] Step B2: β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and DMF are mixed evenly, reacted at a speed of 150 r / min and a temperature of 70°C for 3 hours, and then a sodium hydroxide solution is added, the temperature is raised to 80°C, and the reaction is carried out for 5 hours to obtain epoxy cyclodextrin. Epoxy cyclodextrin, aspartic acid and DMF are mixed evenly, reacted at a speed of 300 r / min, a temperature of 40°C and a pH value of 11 for 6 hours, and the pH is adjusted to be acidic to obtain modified cyclodextrin;
[0057] Step B3: Mix the modified cyclodextrin, lithium hydroxide and DMF, stir for 1.5 hours at a speed of 500 r / min and a temperature of 25°C to obtain a precursor, mix the modified boron nitride, tetraethyl orthosilicate, precursor, DMF and ethanol evenly, stir and add deionized water and hydrochloric acid at a speed of 150 r / min and a temperature of 70°C, react for 3 hours, add tetrabutyl titanate, continue to react for 4 hours, heat to 130°C, and keep warm for 2 hours to obtain a modified filler.
[0058] The amount ratio of hexagonal boron nitride, sodium hydroxide and ethanol described in step B1 is 1g:15g:80mL, and the amount ratio of hydroxyboron nitride and triethoxypropyl isocyanate is 1g:32mL.
[0059] The amount ratio of β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution in step B2 is 3g:1g:0.5g:30mL, the mass fraction of the sodium hydroxide solution is 10%, and the molar ratio of the epoxy group on the epoxycyclodextrin to aspartic acid is 1:1.
[0060] The amount ratio of the modified cyclodextrin, lithium hydroxide and DMF described in step B3 is 1g:8g:20mL, the amount ratio of modified boron nitride, tetraethyl orthosilicate, precursor, deionized water, hydrochloric acid solution and tetrabutyl titanate is 1g:80mmol:3g:10mL:3mL:20mmol, and the mass fraction of the hydrochloric acid solution is 1.5%.
[0061] Comparative Example 1: Compared with Example 1, this comparative example uses a modified substrate as a tile, and the remaining steps are the same.
[0062] Comparative Example 2: Compared with Example 1, no modified filler was added in this comparative example, and the remaining steps were the same.
[0063] Comparative Example 3: Compared with Example 1, no precursor was added in this comparative example, and the remaining steps were the same.
[0064] Comparative Example 4: Compared with Example 1, tetrabutyl titanate was not added in this comparative example, and the remaining steps were the same.
[0065] The anti-fouling grade of the tiles prepared in Examples 1-3 and Comparative Examples 1-4 was tested according to the standard of GB / T3810.14-2016, and the anti-slip coefficient during wet dynamic friction was tested according to the standard of GB / T4100-2015. The test results are shown in Table 1 below.
[0066] Table 1
[0067]
[0068] It can be seen from the above table that the present invention has a good anti-fouling and anti-slip effect.
[0069] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A production process for anti-slip and anti-fouling tiles, characterized in that: The specific steps include: Step A1: mixing and ball-milling the modified filler, silicon carbide and deionized water to obtain a composite material, mixing the composite material, tetraethyl orthosilicate and ethanol, stirring, adding ammonia water and deionized water, reacting, and aging to obtain a composite sol; Step A2: soaking the tile substrate in deionized water, ultrasonically treating it, taking it out and soaking it in acetone, ultrasonically treating it, taking it out and soaking it in ethanol, ultrasonically treating it, taking it out and drying it to prepare a pretreated substrate; Step A3: soaking the pretreated substrate in the composite sol, performing an immersion and pulling treatment, and then drying the substrate. After repeated immersion and pulling and drying, the substrate is sintered to obtain a modified substrate. Heptafluorodecyltrimethoxysilane and ethanol are mixed evenly, and the modified substrate is soaked therein. Deionized water is added, and the substrate is ultrasonically treated. The substrate is taken out and dried to obtain an anti-slip and anti-fouling tile. The mass ratio of the modified filler, silicon carbide and deionized water described in step A1 is 1:1:0.8, and the amount ratio of the composite material, tetraethyl orthosilicate, ethanol, ammonia water and deionized water is 1g:5mL:15mL:10mL:8mL; The volume ratio of heptadecafluorodecyltrimethoxysilane, ethanol and deionized water in step A3 is 1:10:3; The modified filler is prepared by the following steps: Step B1: mixing hexagonal boron nitride, sodium hydroxide and ethanol to react to obtain hydroxy boron nitride, and mixing hydroxy boron nitride, isocyanatepropyltriethoxysilane and DMF to react to obtain modified boron nitride; Step B2: After β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and DMF are mixed for reaction, sodium hydroxide solution is added, and the temperature is raised to react to obtain epoxy cyclodextrin; epoxy cyclodextrin, aspartic acid and DMF are mixed for reaction, and the pH is adjusted to be acidic to obtain modified cyclodextrin; Step B3: the modified cyclodextrin, lithium hydroxide and DMF are mixed and stirred to obtain a precursor, the modified boron nitride, tetraethyl orthosilicate, the precursor, DMF and ethanol are mixed and stirred, and deionized water and hydrochloric acid are added, and tetrabutyl titanate is added after the reaction, and the reaction is continued, and the temperature is raised and kept to obtain a modified filler; The amount ratio of hexagonal boron nitride, sodium hydroxide and ethanol in step B1 is 1g:15g:80mL, and the amount ratio of hydroxyboron nitride and triethoxypropyl isocyanatesilane is 1g:32mL; The amount ratio of β-cyclodextrin, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution in step B2 is 3g:1g:0.5g:30mL, and the molar ratio of the epoxy group on the epoxycyclodextrin to aspartic acid is 1:1; The modified cyclodextrin, lithium hydroxide and DMF in step B3 are used in a ratio of 1 g:8 g:20 mL, and the modified boron nitride, tetraethyl orthosilicate, precursor, deionized water, hydrochloric acid solution and tetrabutyl titanate are used in a ratio of 1 g:80 mmol:3 g:10 mL:3 mL:20 mmol.
2. A non-slip and anti-fouling tile, characterized in that: Prepared according to the production process of claim 1.