A high-strength and plastic copper-containing super ferrite stainless steel and its production process

By adding an appropriate amount of copper and appropriate process to super ferrite stainless steel, the corrosion and grain coarse problems are solved, the strength and corrosion resistance of the material are improved, and the super ferrite with high strength and high toughness is achieved Production of stainless steel.

CN118703752BActive Publication Date: 2024-11-12TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411203832.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Super ferrite stainless steel has serious corrosion problems during its preparation and service. High-temperature annealing treatment leads to roughening of grains, reducing the mechanical properties of the material. When the Cr element content is too high, the σ phase is formed, resulting in a decrease in corrosion resistance.

Method used

The production process of high-strength plastic copper-containing super ferrite stainless steel is adopted to obtain copper-containing super ferrite stainless steel ingots through smelting, and homogenize hot rolling, solid solution treatment, cold rolling and annealing to control the combination of Cr, Mo and Fe. It can hinder the precipitation of σ phase, refine the grains, improve the strength and corrosion resistance of the material.

Benefits of technology

It significantly improves the yield strength, tensile strength and elongation of stainless steel, reduces production costs, enhances the toughness and ductility of the material, and maintains good corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention belongs to the field of iron and steel metallurgy technology, specifically a high-strength plastic copper-containing super ferritic stainless steel and its production process, by adding an appropriate amount of Cu in the super ferritic stainless steel, reducing the use of the precious element Ni, so that the production cost is reduced; matching a suitable production process, can reduce the binding energy of Cr, Mo and Fe, while hindering their segregation to the grain boundary, the σ phase precipitation dynamics in the steel is significantly reduced, thereby significantly improving the strength and hardness of the stainless steel, and promoting the refinement of metal grains, making up for the defects of the steel, so that the stainless steel has higher toughness and ductility. The yield strength of the high-strength plastic copper-containing super ferritic stainless steel of the present invention is 500~610MPa, the tensile strength is 600~660MPa, the elongation is 25~29%, and the corrosion potential is -0.25V~-0.35V.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, in particular to a high-strength and plastic copper-containing super ferrite stainless steel and a production process thereof. Background Art

[0002] Super ferritic stainless steel is a kind of resource-saving high-performance material with excellent corrosion resistance, good thermal conductivity and mechanical properties. The pitting equivalent PREN value is usually above 35. It is a potential low-cost material to replace titanium and copper for the manufacture of cooling pipes with seawater as the medium. The corrosion resistance of high-grade ferritic stainless steel is equivalent to that of super austenitic stainless steel and nickel-based alloy. However, at present, super ferritic stainless steel has serious corrosion problems in the preparation and service process, and its production is difficult, and the wide application of the product is limited. Studies have found that Cr and Mo elements significantly improve the recrystallization temperature, pitting resistance and sulfuric acid corrosion resistance of the material. Therefore, super ferritic stainless steel has an extremely high Cr content (26~30wt%) and extremely excellent corrosion resistance. However, when the Cr content exceeds 40wt%, a certain amount of σ phase will be formed in the steel. The formation of σ phase will form a chromium-poor area on the surface of the material, resulting in a decrease in corrosion resistance. In the prior art, in order to avoid the large-scale precipitation of unfavorable precipitated phases (such as σ phase and χ phase) resulting in the formation of chromium-depleted areas on the material surface, a general treatment method is to use high-temperature annealing. However, high-temperature annealing will also cause the problem of grain coarsening of super ferritic stainless steel, resulting in a decrease in the mechanical properties of super ferritic stainless steel. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a high-strength and ductile copper-containing super ferrite stainless steel and its production process.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A production process of high-strength and ductile copper-containing super ferrite stainless steel comprises the following steps:

[0006] S1. Smelting to obtain an ingot of copper-containing super ferritic stainless steel; the copper-containing super ferritic stainless steel has a Cu content of 0.5-1.5wt%, a Cr content of 25.0-28.0wt%, a Mo content of 1.0-4.0wt%, and a Ni content of 1.00-3.00%;

[0007] S2, hot rolling is immediately performed to obtain a plate after the ingot is homogenized;

[0008] S3, the plate is subjected to solution treatment, cooled immediately after the heat preservation, and then the surface oxide scale is removed;

[0009] S4, the plate after solution treatment is subjected to multiple cold rolling to obtain a cold rolled plate;

[0010] S5. The cold-rolled sheet is annealed and then air-cooled to room temperature to obtain high-strength and ductile copper-containing super ferritic stainless steel.

[0011] As a preferred solution of the production process of a high-strength and ductile copper-containing super ferrite stainless steel described in the present invention, wherein: in the step S2, the homogenization temperature is 1210-1270°C, and the homogenization time is 4-5h.

[0012] As a preferred solution of the production process of a high-strength and ductile copper-containing super ferritic stainless steel described in the present invention, wherein: in the step S2, the starting rolling temperature is ≥1210°C, the final rolling temperature is ≥800°C; the single-pass hot rolling reduction is <25%, and the total reduction is ≥65%.

[0013] As a preferred solution of the production process of a high-strength and ductile copper-containing super ferrite stainless steel described in the present invention, wherein: in the step S3, the temperature of the solution treatment is 1050-1100°C, and the holding time is 0.5-2h.

[0014] As a preferred solution of the production process of a high-strength and ductile copper-containing super ferrite stainless steel described in the present invention, wherein: in the step S3, oil cooling or water cooling is adopted for cooling.

[0015] As a preferred solution of the production process of a high-strength and ductile copper-containing super ferrite stainless steel described in the present invention, wherein: in the step S4, 7 cold rolling passes are performed, and the total cold rolling reduction is 65-75%.

[0016] As a preferred solution of the production process of a high-strength and ductile copper-containing super ferrite stainless steel described in the present invention, wherein: in the step S5, the annealing temperature is 950-1100°C, and the annealing time is 2-240 min.

[0017] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0018] A high-strength and ductile copper-containing super ferrite stainless steel is prepared by adopting the above-mentioned production process of the high-strength and ductile copper-containing super ferrite stainless steel.

[0019] As a preferred embodiment of the high-strength, ductile, copper-containing super ferritic stainless steel described in the present invention, the high-strength, ductile, copper-containing super ferritic stainless steel has a yield strength of 500-610 MPa, a tensile strength of 600-660 MPa, an elongation of 25-29%, and a corrosion potential of -0.25 V to -0.35 V.

[0020] As a preferred embodiment of the high-strength and ductile copper-containing super ferritic stainless steel described in the present invention, the composition of the high-strength and ductile copper-containing super ferritic stainless steel, in terms of mass percentage, includes: Cr 25.0-28.0%, Mo 1.0-4.0%, Ni 1.00-3.00%, C≤0.030%, N≤0.040%, Nb 0.05-0.65%, Ti 0.15-0.45%, Cu 0.5-1.5%, Mn≤1.00%, Si≤1.00%, S≤0.030%, P≤0.040%, and the rest are Fe and unavoidable impurities; and satisfies Cr+3.3×Mo≥34%.

[0021] The beneficial effects of the present invention are as follows:

[0022] The present invention proposes a high-strength and plastic copper-containing super ferritic stainless steel and its production process. By adding an appropriate amount of Cu to the super ferritic stainless steel, the use amount of the precious element Ni is reduced, so that the production cost is reduced; matching a suitable production process can reduce the binding energy of Cr, Mo and Fe, and at the same time hinder their segregation to the grain boundary, and the kinetics of σ phase precipitation in the steel is significantly reduced, thereby significantly improving the strength and hardness of the stainless steel, and promoting the refinement of metal grains, compensating for the defects of the steel, and making the stainless steel have higher toughness and ductility. The high-strength and plastic copper-containing super ferritic stainless steel of the present invention has a yield strength of 500~610MPa, a tensile strength of 600~660MPa, an elongation of 25~29%, and a corrosion potential of -0.25V~-0.35V. DETAILED DESCRIPTION

[0023] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] According to one aspect of the present invention, the present invention provides the following technical solution:

[0025] A production process of high-strength and ductile copper-containing super ferrite stainless steel comprises the following steps:

[0026] S1. Smelting to obtain an ingot of copper-containing super ferritic stainless steel; the copper-containing super ferritic stainless steel has a Cu content of 0.5-1.5wt%, a Cr content of 25.0-28.0wt%, a Mo content of 1.0-4.0wt%, and a Ni content of 1.00-3.00%;

[0027] S2, hot rolling is immediately performed to obtain a plate after the ingot is homogenized;

[0028] S3, the plate is subjected to solution treatment, cooled immediately after the heat preservation, and then the surface oxide scale is removed;

[0029] S4, the plate after solution treatment is subjected to multiple cold rolling to obtain a cold rolled plate;

[0030] S5. The cold-rolled sheet is annealed and then air-cooled to room temperature to obtain high-strength and ductile copper-containing super ferritic stainless steel.

[0031] The present invention adds an appropriate amount of copper to the super ferritic stainless steel, which can improve the wear resistance and corrosion resistance of the super ferritic stainless steel, because on the one hand, it can achieve fine grain strengthening and precipitation strengthening effects, greatly improving the yield strength of TRIP high-strength steel; on the other hand, the copper element is concentrated at the grain boundary, which can hinder the aggregation and growth of vacancies at the interface, which is conducive to the pinning of corrosion products into the matrix, improving the adhesion between the passivation film and the matrix, and promoting the formation of a continuous and dense passivation film. The passivation film can adhere to the surface of the material to prevent the surface of the material from being further corroded, so that the super ferritic stainless steel has excellent corrosion resistance.

[0032] Preferably, in step S1, the raw materials are melted in a vacuum induction furnace and then cast to obtain an ingot. Super ferritic stainless steel has a body-centered cubic ferrite structure in the entire temperature range due to its low (C+N) content, and there is no phase change. The cast coarse grains can only be refined by controlling the deformation degree and deformation temperature during forging and rolling. After the ingot is air-cooled to room temperature, the outer oxide scale is removed: the alloy elements are added in the form of high-purity pure metal raw materials.

[0033] Preferably, in step S2, the homogenization temperature is 1210-1270°C, and the homogenization time is 4-5h. Specifically, the homogenization temperature can be, for example, any one of 1210°C, 1220°C, 1230°C, 1240°C, 1250°C, 1260°C, 1270°C, or a range between any two thereof; the homogenization temperature can be, for example, any one of 4h, 4h10min, 4h20min, 4h30min, 4h40min, 4h50min, 5h, or a range between any two thereof; the starting rolling temperature is ≥1210°C, the finishing rolling temperature is ≥800°C; the single-pass hot rolling reduction is <25%, and the total reduction is ≥65%. Specifically, the start rolling temperature can be, for example, any one of 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, 1250°C or any range between two thereof: the final rolling temperature can be, for example, any one of 800°C, 820°C, 840°C, 860°C, 880°C, 900°C or any range between two thereof: the single hot rolling reduction can be, for example, any one of 20%, 15%, 10%, 5% or any range between two thereof. During the rolling process, the surface defects of the rolled plate caused by the excessively low local temperature of the rolled plate or the increased rolling load due to the excessive reduction rate of individual passes should be avoided. In order to avoid copper brittleness and microcracks on the surface, a smaller reduction rate should be used, the single hot rolling reduction is less than 25%, and the multi-pass rolling is performed, and the total reduction is guaranteed to be above 65% to ensure the complete fragmentation of the as-cast structure. The control of the reduction can effectively control the uniformity of the temperature and deformation of the slab.

[0034] Preferably, in step S3, the temperature of the solution treatment is 1050-1100°C, and the holding time is 0.5-2h. The high-strength and plastic copper-containing super ferritic stainless steel is further improved in performance by solution treatment. In the solution treatment, the alloying elements in the copper-containing super ferritic stainless steel will dissolve in the ferrite matrix to form a solid solution. The solution treatment will promote the dissolution of the precipitated phase and increase the strength and plasticity of the solid solution, thereby improving the performance of the stainless steel. In addition, the solution treatment can also eliminate the residual stress in the stainless steel and improve its corrosion resistance. Specifically, the temperature of the solution treatment can be, for example, any one of 1050°C, 1060°C, 1070°C, 1080°C, 1090°C, 1100°C or any range between two of them: the holding time can be, for example, but not limited to, any one of 0.5h, 1h, 1.5h, 2h or any range between two of them; oil cooling or water cooling is used for cooling.

[0035] Preferably, in step S4, 7 cold rolling passes are performed, and the total cold rolling reduction is 65-75%. Specifically, the total cold rolling reduction can be, for example, any one of 65%, 68%, 70%, 72%, 75%, or a range between any two of them.

[0036] Preferably, in step S5, the annealing temperature is 950-1100°C, and the annealing time is 2-240 min. On the basis of effectively eliminating the residual stress after cold rolling, the grains are further refined to promote the precipitation of copper-rich phase. The cold-rolled deformed structure is mainly statically recovered during the low-temperature annealing process, and a large number of subgrain boundaries are formed in the crystals; as the annealing time increases, a large number of "grain clusters" are formed in the intracrystalline shear bands. During the annealing process, the cold-rolled structure is mainly recrystallized, and nucleation is preferentially formed at the shear band position during the recrystallization process. The "grain clusters" formed during the recovery process gradually develop into recrystallization cores. After annealing below 1050°C, as the annealing time increases, the size of the recrystallized grains is relatively stable. Specifically, the annealing temperature can be, for example, but not limited to, any one of 950°C, 980°C, 1010°C, 1040°C, 1070°C, 1100°C, or a range between any two of them; the annealing time can be, for example, but not limited to, any one of 2 min, 30 min, 60 min, 90 min, 120 min, 150 min, 180 min, 210 min, 240 min, or a range between any two of them.

[0037] According to another aspect of the present invention, the present invention provides the following technical solution:

[0038] A high-strength and ductile copper-containing super ferrite stainless steel is prepared by adopting the above-mentioned production process of the high-strength and ductile copper-containing super ferrite stainless steel.

[0039] Preferably, the high-strength plastic copper-containing super ferritic stainless steel has a yield strength of 500-610 MPa, a tensile strength of 600-660 MPa, an elongation of 25-29%, and a corrosion potential of -0.25V--0.35V.

[0040] Preferably, the composition of the high-strength and ductile copper-containing super ferritic stainless steel includes, by mass percentage, Cr25.0~28.0%, Mo 1.0~4.0%, Ni 1.00~3.00%, C≤0.030%, N≤0.040%, Nb 0.05~0.65%, Ti0.15~0.45%, Cu 0.5~1.5%, Mn≤1.00%, Si≤1.00%, S≤0.030%, P≤0.040%, and the rest are Fe and unavoidable impurities; and satisfies Cr+3.3×Mo≥34%.

[0041] Cr: It is one of the key elements of stainless steel. It forms a dense chromium oxide (Cr2O3) film, called a passivation film, which can prevent further oxidation and corrosion and provide corrosion resistance. The addition of chromium can greatly improve the corrosion resistance of the material. When the content of Cr element exceeds 40wt%, a certain amount of σ phase will be formed in the steel, making the super ferrite stainless steel embrittled. Therefore, the higher the Cr content, the worse the toughness of the steel and the higher the brittle transition temperature. The present invention reduces the Cr content and controls the Cr content to 25.0~28.0wt%.

[0042] Si: The addition of silicon can reduce the stacking fault energy of the alloy and promote the formation of twins, thereby improving the mechanical properties of the alloy. Silicon is an important corrosion-resistant element. The addition of silicon can significantly improve the strength and corrosion resistance of stainless steel and help inhibit intergranular corrosion. The present invention controls Si≤1.00wt%.

[0043] Mn: As an alloying element added to stainless steel, it can improve strength, hardness and wear resistance, and help reduce sensitization tendency during heat treatment. It can also reduce the stacking fault energy of the material and improve the deformation strengthening ability of the material. The addition of Mn element can make the steel achieve the effect of processing strengthening in the subsequent cold working process. The present invention controls Mn≤1.00wt%.

[0044] Ni: Improves the corrosion resistance of stainless steel and increases its acid and alkali resistance. In addition, nickel also helps to improve the strength and plasticity of the material. However, Ni is one of the more expensive alloy elements, and reducing the Ni content can significantly reduce costs. The present invention controls the Ni content to 1.00-3.00wt%.

[0045] Mo: Increases the corrosion resistance of stainless steel, especially in acidic environments and chloride media. In addition, molybdenum can also improve the strength, hardness and high temperature resistance of stainless steel. However, it is easy to form harmful phases such as laves phase and σ phase, so it should be controlled. The present invention controls the Mo content to 1.0~4.0wt%.

[0046] Nb: By combining with carbon to form niobium carbide, carbon can be stabilized, the precipitation of ferrite phase can be inhibited, and corrosion resistance can be improved. In addition, niobium can also improve the strength, plasticity and high temperature resistance of the material. The present invention controls the Nb content to be 0.05-0.65wt%.

[0047] Ti: Combined with carbon to form titanium carbide, it can stabilize carbon, prevent excessive precipitation of ferrite, and improve corrosion resistance. In addition, titanium also helps to improve the strength and high temperature resistance of the material. The present invention controls the Ti content to 0.15-0.45wt%.

[0048] Cu: The effect of adding copper is as described above, but the copper content has an important influence on the performance of stainless steel. The copper content should not exceed 1.5wt%, otherwise the super ferritic stainless steel will become brittle. Therefore, considering comprehensively, the Cu content should be controlled in the range of 0.5~1.5wt%. Specifically, the Cu content can be, for example, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, any one of them or the range between any two of them; this low copper content alloy can provide a certain strengthening effect while maintaining the good plasticity and elongation of super ferritic stainless steel to ensure a balance between formability and corrosion resistance.

[0049] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0050] The chemical compositions of the super ferrite stainless steels of the embodiments and comparative examples of the present invention are shown in Table 1.

[0051] Table 1 Chemical composition of super ferrite stainless steel of each embodiment and comparative example (wt%)

[0052]

[0053] The main production process parameters of the super ferrite stainless steel of each embodiment of the present invention and the comparative example are shown in Table 2.

[0054] Table 2 Production process parameters of super ferrite stainless steel in various embodiments and comparative examples

[0055]

[0056] The properties of the super ferrite stainless steel of each embodiment of the present invention and the comparative example are shown in Table 3.

[0057] Table 3 Properties of super ferrite stainless steel of various embodiments and comparative examples

[0058]

[0059] The present invention reduces the use amount of the precious element Ni by adding an appropriate amount of Cu to the super ferritic stainless steel, thereby reducing the production cost; matching a suitable production process can reduce the binding energy of Cr, Mo and Fe, while hindering their segregation to the grain boundary, and significantly reducing the kinetics of σ phase precipitation in the steel, thereby significantly improving the strength and hardness of the stainless steel, and promoting the refinement of metal grains, compensating for the defects of the steel, and making the stainless steel have higher toughness and ductility. The high-strength plastic copper-containing super ferritic stainless steel of the present invention has a yield strength of 500~610MPa, a tensile strength of 600~660MPa, an elongation of 25~29%, and a corrosion potential of -0.25V~-0.35V.

[0060] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A production process of high-strength and ductile copper-containing super ferrite stainless steel, characterized in that: The steps include: S1. Smelting to obtain an ingot of copper-containing super ferrite stainless steel; S2. After the ingot is homogenized, it is immediately hot rolled to obtain a plate; the homogenization temperature is 1210~1270℃, and the final rolling temperature is ≥800℃; S3, the plate is subjected to solution treatment, cooled immediately after the insulation, and then the surface oxide scale is removed; the temperature of the solution treatment is 1050~1100℃; S4, the plate after solution treatment is subjected to multiple cold rolling to obtain a cold rolled plate; S5, the cold-rolled sheet is annealed at a temperature of 950-1100°C, and then air-cooled to room temperature to obtain high-strength and plastic copper-containing super ferrite stainless steel; The composition of the copper-containing super ferritic stainless steel, in terms of mass percentage, includes: Cr 25.0~28.0%, Mo 1.0~4.0%, Ni 1.00~3.00%, C≤0.030%, N≤0.040%, Nb 0.05~0.65%, Ti 0.15~0.45%, Cu 1.1~1.5%, Mn≤1.00%, Si≤1.00%, S≤0.030%, P≤0.040%, and the rest is Fe and unavoidable impurities; and satisfies Cr+3.3×Mo≥34%; Its yield strength is 500~610MPa, tensile strength is 600~660MPa, elongation is 25~29%, and corrosion potential is -0.25V~-0.35V.

2. The production process of high-strength and ductile copper-containing super ferrite stainless steel according to claim 1, characterized in that: In step S2, the homogenization time is 4 to 5 hours.

3. The production process of high-strength and ductile copper-containing super ferrite stainless steel according to claim 1, characterized in that: In the step S2, the rolling temperature is ≥ 1210°C.

4. The production process of high-strength and ductile copper-containing super ferrite stainless steel according to claim 1, characterized in that: In the step S2, the hot rolling reduction in a single pass is less than 25%, and the total hot rolling reduction is ≥ 65%.

5. The production process of high-strength and ductile copper-containing super ferrite stainless steel according to claim 1, characterized in that: In step S3, the insulation time is 0.5 to 2 hours.

6. The production process of high-strength and ductile copper-containing super ferrite stainless steel according to claim 1, characterized in that: In step S4, the total cold rolling reduction is 65-75%.

7. The production process of high-strength and ductile copper-containing super ferrite stainless steel according to claim 1, characterized in that: In step S5, the annealing time is 2 to 240 minutes.

8. A high-strength, ductile, copper-containing super ferrite stainless steel, characterized in that: The high-strength and plastic copper-containing super ferrite stainless steel is prepared by the production process of any one of claims 1 to 7.