Sulfide solid electrolyte and preparation method and application thereof
By adjusting the ratio and solvent combination of Li2S, P2S5 and LiX in the liquid phase method, forming a homogeneous solution and drying and calcining it, the problems of heterogeneous reactions and low efficiency in the liquid phase method are solved, and high purity and high lithium are achieved Rapid preparation and mass production of sulfide solid-state electrolytes with ionic conductivity.
Patent Information
- Application Number
- CN202410872610.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-09-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When the existing liquid phase method is used to prepare sulfide solid electrolytes with high purity and high lithium ion conductivity, there are problems with the heterogeneous reaction process and low preparation efficiency, making it difficult to achieve mass production.
By mixing Li2S, P2S5 and LiX in specific proportions in different solvents to form a homogeneous solution, drying and calcining it under an inert atmosphere, reducing raw material residues and the formation of Li3PO4, and improving the purity of the electrolyte and lithium ion conductivity.
The rapid preparation of sulfide solid electrolyte with high purity and high lithium ion conductivity is achieved, which improves the preparation efficiency and has the feasibility of mass production.
Smart Images

Figure CN118712466A
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a sulfide solid electrolyte and a preparation method and application thereof. Background Art
[0002] In the field of lithium-ion batteries, it is widely recognized that the use of solid electrolytes instead of electrolytes containing flammable organic solvents not only simplifies safety measures, but also brings many advantages in terms of manufacturing costs and production efficiency. It is particularly noteworthy that sulfide-based solid electrolytes, such as Li x PS x 、Li6PS5X(X=Cl,Br or I)、Li x MP x S x (M=Ge, Sn, Si or Al), etc., have excellent electrical conductivity (ie, lithium ion conductivity), and play an important role in improving battery power. Among them, Li6PS5X, which has low cost and high electrical conductivity, has attracted much attention, and there are currently a variety of preparation methods to choose from. For example, one method is to achieve solid-phase synthesis by mechanically grinding and heat treating the raw materials of the electrolyte material under an inert atmosphere; another method is to place the solid electrolyte raw materials in a solvent for reaction to complete the liquid phase synthesis of the electrolyte. The solid-phase method can produce sulfide solid electrolytes with higher purity and ionic conductivity, but its preparation efficiency is low and it is difficult to achieve mass production. In contrast, the liquid-phase method is universal and scalable, and is easy to synthesize on a large scale, but the existing liquid-phase method has a heterogeneous reaction process. The key to its synthesis is the need for stirring for 24 hours or even longer, and the preparation efficiency needs to be further improved. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a sulfide solid electrolyte and a preparation method and application thereof. The preparation method of the present invention can reduce the residual raw materials and the formation of Li3PO4, and can quickly prepare a sulfide solid electrolyte with high purity and high lithium ion conductivity.
[0004] In a first aspect, the present invention provides a method for preparing a sulfide solid electrolyte, comprising the following steps:
[0005] Mix Li2S, P2S5 and solvent A and stir once to obtain solution A;
[0006] Mix Li2S, LiX and solvent B, then add elemental sulfur or add elemental sulfur and P2S5, and stir for a second time to obtain solution B, wherein X is selected from Cl, Br or I;
[0007] The solution B is added to the solution A and stirred three times to obtain a Li-PSX homogeneous solution;
[0008] The Li-PSX homogeneous solution is dried to remove solvent A and solvent B to obtain a precursor powder;
[0009] calcining the precursor powder under inert gas conditions to obtain the sulfide solid electrolyte;
[0010] In the solution A, the molar ratio of Li2S to P2S5 is 1:(1-1.5), for example, it can be any point value among 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, or a range value between two arbitrary point values;
[0011] In the Li-PSX homogeneous solution, the molar ratio of Li2S, P2S5 and LiX is 5:(1.05-1.5):2, for example, it can be any point value among 5:1.05:2, 5:1.06:2, 5:1.07:2, 5:1.08:2, 5:1.09:2, 5:1.1:2, 5:1.2:2, 5:1.3:2, 5:1.4:2, and 5:1.5:2, or a range value between two arbitrary point values.
[0012] In some embodiments of the present invention, in the solution B, the molar ratio of Li2S to LiX is (3.5-4.5):2, for example, it can be any point value among 3.5:2, 3.6:2, 3.7:2, 3.8:2, 3.9:2, 4:2, 4.1:2, 4.2:2, 4.3:2, 4.4:2, and 4.5:2, or a range value between two arbitrary point values.
[0013] In some embodiments of the present invention, in the Li-PSX homogeneous solution, the molar ratio of Li2S, P2S5, LiX and elemental sulfur is 5:(1.05-1.5):2:(0.5-2.5), preferably 5:(1.05-1.5):2:(1-2), and more preferably 5:1.1:2:(1-2).
[0014] In some embodiments of the present invention, the solvent A is a polar aprotic solvent, and the solvent A includes at least one of acetonitrile, tetrahydrofuran, tetrahydropyrrole, ethylenediamine, dimethylamine and dimethylformamide.
[0015] Specifically, polar aprotic solvents will not cause violent decomposition reactions in raw materials and precursors; acetonitrile is preferred as solvent A because it is a polar aprotic solvent that will not cause violent decomposition reactions in raw materials and precursors. In addition, since acetonitrile does not contain oxygen, sulfur atoms in the raw materials and precursors cannot undergo exchange reactions with oxygen.
[0016] Specifically, when the molar ratio of P2S5 to Li2S is 1:1, it has high solubility in polar solvents such as acetonitrile. Solution A (Li-PS clear solution) obtained at this ratio has high reactivity, which helps to quickly react with Li2S and LiX in solution B, and can greatly shorten the stirring reaction time.
[0017] In some embodiments of the present invention, the solvent B is an organic solvent containing a hydroxyl group or a thiol group, and the solvent B includes at least one of methanol, ethanol, isopropanol, ethanethiol and ethanedithiol, preferably ethanol.
[0018] Specifically, in the Li-PSX homogeneous solution obtained by the present invention, the molar ratio of Li2S, P2S5 and LiX is 5: (1.05-1.5): 2, indicating that the proportion of P2S5 is higher than the target molar ratio (i.e., Li2S: P2S5: LiX = 5: 1: 2); in order to ensure that the Li2S in solvent B has a high reactivity, it is necessary to use an alcohol solvent to completely dissolve it. Phosphorus pentasulfide and alcohol solvents undergo a thioesterification reaction to form thiohydric anhydride or thioether. The present invention can reduce the impact of side reactions between phosphorus pentasulfide and alcohol solvents by adding a certain molar ratio of phosphorus pentasulfide to solvent A or solvent B, reduce the content of Li2S and LiX impurities in the target sulfide solid electrolyte, and thus improve lithium ion conductivity.
[0019] In addition, the present invention adds additional elemental sulfur to solvent B for two benefits: first, it inhibits sulfur loss caused by the volatilization of part of the sulfur element during drying and calcination; second, elemental sulfur can form easily soluble lithium polysulfide with lithium sulfide, and the addition of excess elemental sulfur can promote the dissolution of lithium sulfide, thereby reducing the amount of solvent B (alcohol solvent) required, and further reducing the side reaction between phosphorus pentasulfide and alcohol solvent. Therefore, adding elemental sulfur can also reduce the impurities in the electrolyte to a certain extent and improve its lithium ion conductivity.
[0020] In some embodiments of the present invention, the first stirring time is 0.5 to 3 hours; the second stirring time is 0.5 to 2 hours; the third stirring time is 0.5 to 4 hours; and the stirring speed is 600 to 1000 rpm.
[0021] In some embodiments of the present invention, the drying temperature is 60 to 180° C.; and / or the drying time is 3 to 12 hours.
[0022] In some embodiments of the present invention, the calcination temperature is 300-600° C.; and / or the calcination time is 2-12 hours.
[0023] In some embodiments of the present invention, after the three stirrings, a step of centrifugal separation and collecting a supernatant is further included, and the supernatant is a Li-PSX homogeneous solution.
[0024] In some embodiments of the present invention, the rotation speed of the centrifugal separation is 3000-10000 rpm; and / or the time of the centrifugal separation is 10-30 min.
[0025] In a second aspect, the present invention provides a sulfide solid electrolyte, which is prepared by the preparation method described in the first aspect of the present invention.
[0026] In some embodiments of the present invention, the lithium ion conductivity of the sulfide solid electrolyte is greater than 1.3 mS·cm -1 , can reach 3.22mS·cm -1 .
[0027] In some embodiments of the present invention, the D50 particle size of the sulfide solid electrolyte is 4 to 7 μm.
[0028] According to a third aspect of the present invention, a solid-state battery is provided, wherein the solid-state battery comprises the sulfide solid electrolyte according to the second aspect of the present invention.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0030] (1) The present invention utilizes a liquid phase method to dissolve raw material components in specific proportions in different solvents (solvent A and solvent B), first prepare two homogeneous solutions (solution A and solution B), then mix solution A and solution B, and then dry and calcine them, thereby realizing the rapid manufacture of sulfide solid electrolytes.
[0031] (2) In the preparation method of the present invention, by adjusting the ratio of P2S5, LiX and Li2S and different solvent combinations, and adding elemental sulfur, the residual raw materials and the formation of Li3PO4 impurity phase can be reduced, thereby improving the purity of the prepared sulfide solid electrolyte.
[0032] (3) The organic solvent used has excellent solubility or dispersion ability for the precursor of the target sulfide solid electrolyte, ensuring the uniformity of the precursor composition and realizing the liquid phase preparation of high-purity sulfide solid electrolyte.
[0033] (4) The method of preparing the sulfide solid electrolyte by dissolving the elements constituting the sulfide solid electrolyte into a specific solvent is simple and quick, and has the characteristics of high efficiency and mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The XRD spectra of the embodiments and comparative examples of the present invention are shown in FIG.
[0035] Figure 2 This is a low-magnification scanning electron microscope image of the sulfide solid electrolyte powder prepared in Example 2 of the present invention;
[0036] Figure 3 This is a high-magnification scanning electron microscope image of the sulfide solid electrolyte powder prepared in Example 2 of the present invention;
[0037] Figure 4 This is a scanning electron microscope image of a cross section of a sulfide solid electrolyte pellet obtained in Example 2 of the present invention;
[0038] Figure 5 The AC impedance spectra of the sulfide solid electrolytes prepared in the examples and comparative examples of the present invention. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below by specific examples. The raw materials, reagents or devices used in the examples can be obtained from conventional commercial sources or by prior art methods unless otherwise specified. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0040] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±1%, for example, about 1 actually means 1±1%×1.
[0041] Example 1: Preparation of Li6PS5Cl sulfide solid electrolyte
[0042] The Li6PS5Cl sulfide solid electrolyte of this embodiment is prepared by the preparation method of the following steps:
[0043] (1) 0.345 g of Li2S and 1.667 g of P2S5 (i.e., a molar ratio of about 1:1) were mixed with 25 mL of acetonitrile and stirred at 600 rpm for 2 h at room temperature (25 °C) to obtain a homogeneous solution A;
[0044] (2) 1.379 g of Li2S and 0.636 g of LiCl (i.e., a molar ratio of about 4:2) were dissolved in 50 mL of anhydrous ethanol, and 0.167 g of P2S5 and 0.241 g of elemental sulfur powder were additionally added, and the mixture was stirred at 600 rpm for 30 min until the solution was homogeneous and stable, thereby obtaining a homogeneous solution B;
[0045] (3) slowly adding the homogeneous solution B to the homogeneous solution A, stirring at 600 rpm for 1 h, and then centrifuging at 4000 rpm for 10 min, collecting the supernatant to obtain a Li-PS-Cl homogeneous solution; the molar ratio of Li2S, P2S5, LiCl and S in the Li-PS-Cl homogeneous solution is about 5:1.1:2:1;
[0046] (4) drying the Li-PS-Cl homogeneous solution under vacuum at 120° C. for 5 h to remove all solvents and obtain a precursor powder;
[0047] (5) The precursor powder was sintered at 550 °C for 5 h under argon to obtain Li6PS5Cl solid electrolyte.
[0048] Example 2: Preparation of Li6PS5Cl sulfide solid electrolyte
[0049] The Li6PS5Cl sulfide solid electrolyte of this embodiment is prepared by the preparation method of the following steps:
[0050] (1) 0.253 g of Li2S and 1.222 g of P2S5 (i.e., a molar ratio of about 1.1:1.1) were mixed with 20 mL of acetonitrile and stirred at 600 rpm for 2 h at room temperature to obtain a homogeneous solution A;
[0051] (2) 0.896 g of Li2S and 0.424 g of LiCl (i.e., a molar ratio of about 3.9:2) were dissolved in 40 mL of anhydrous ethanol, and 0.321 g of elemental sulfur powder was additionally added, and the mixture was stirred at 600 rpm for 30 min until the solution was homogeneous and stable, thereby obtaining a homogeneous solution B;
[0052] (3) slowly adding the homogeneous solution B to the homogeneous solution A, stirring at 600 rpm for 1 h, and then centrifuging at 4000 rpm for 10 min, collecting the supernatant to obtain a Li-PS-Cl homogeneous solution; the molar ratio of Li2S, P2S5, LiCl and S in the Li-PS-Cl homogeneous solution is about 5:1.1:2:2;
[0053] (4) drying the Li-PS-Cl homogeneous solution under vacuum at 120° C. for 5 h to remove all solvents and obtain a precursor powder;
[0054] (5) The precursor powder was sintered at 550 °C for 5 h under argon to obtain Li6PS5Cl solid electrolyte.
[0055] Example 3: Preparation of Li6PS5Br sulfide solid electrolyte
[0056] The Li6PS5Br sulfide solid electrolyte of this embodiment is prepared by the preparation method of the following steps:
[0057] (1) 0.253 g of Li2S and 1.222 g of P2S5 (i.e., a molar ratio of about 1.1:1.1) were mixed with 20 mL of acetonitrile and stirred at 600 rpm for 2 h at room temperature to obtain a homogeneous solution A;
[0058] (2) 0.896 g of Li2S and 0.869 g of LiBr (i.e., a molar ratio of about 3.9:2) were dissolved in 40 mL of anhydrous ethanol, and 0.321 g of elemental sulfur powder was additionally added, and the mixture was stirred at 600 rpm for 30 min until the solution was homogeneous and stable, thereby obtaining a homogeneous solution B;
[0059] (3) slowly adding the homogeneous solution B into the homogeneous solution A, stirring at 600 rpm for 1 h, and then centrifuging at 4000 rpm for 10 min, collecting the supernatant to obtain a Li-PS-Br homogeneous solution; the molar ratio of Li2S, P2S5, LiBr and S in the Li-PS-Br homogeneous solution is about 5:1.1:2:2;
[0060] (4) drying the Li-PS-Br homogeneous solution under vacuum at 120° C. for 5 h to remove all solvents and obtain a precursor powder;
[0061] (5) The precursor powder was sintered at 550 °C for 5 h under argon to obtain Li6PS5Br solid electrolyte.
[0062] Comparative Example 1: Preparation of Li6PS5Cl sulfide solid electrolyte
[0063] The Li6PS5Cl sulfide solid electrolyte of this comparative example is prepared by the preparation method of the following steps:
[0064] (1) 0.345 g of Li2S and 1.667 g of P2S5 (i.e., a molar ratio of about 1:1) were mixed with 25 mL of acetonitrile and stirred at 600 rpm for 2 h at room temperature to obtain a homogeneous solution A;
[0065] (2) 1.379 g of Li2S and 0.636 g of LiCl (i.e., a molar ratio of about 4:2) were dissolved in 80 mL of anhydrous ethanol and stirred at 600 rpm for 30 min until the solution was homogeneous and stable, thereby obtaining a homogeneous solution B;
[0066] (3) slowly adding the homogeneous solution B to the homogeneous solution A, stirring at 600 rpm for 1 h, and then centrifuging at 4000 rpm for 10 min, collecting the supernatant to obtain a Li-PS-Cl homogeneous solution; the molar ratio of Li2S, P2S5 and LiCl in the Li-PS-Cl homogeneous solution is about 5:1:2;
[0067] (4) drying the Li-PS-Cl homogeneous solution under vacuum at 120° C. for 5 h to remove all solvents and obtain a precursor powder;
[0068] (5) The precursor powder was sintered at 550 °C for 5 h under argon to obtain Li6PS5Cl solid electrolyte.
[0069] Comparative Example 2: Preparation of Li6PS5Cl sulfide solid electrolyte
[0070] The Li6PS5Cl sulfide solid electrolyte of this comparative example is prepared by the preparation method of the following steps:
[0071] (1) 1.379 g of Li2S, 1.334 g of P2S5 and 0.509 g of LiCl (i.e., a molar ratio of about 5:1:2) were mixed and dissolved in 80 mL of anhydrous ethanol. The solid phase concentration of the solution was 0.04 g / mL. The mixture was stirred at 600 rpm for 3 h at room temperature to obtain a clear solution.
[0072] (2) drying the solution under vacuum at 100° C. for 6 h to remove all solvents and obtain a precursor powder;
[0073] (3) The precursor powder was sintered at 550 °C for 5 h under argon to obtain Li6PS5Cl solid electrolyte.
[0074] Comparative Example 3: Preparation of Li6PS5Cl sulfide solid electrolyte
[0075] The Li6PS5Cl sulfide solid electrolyte of this comparative example is prepared by the preparation method of the following steps:
[0076] (1) 1.379 g of Li2S and 2.223 g of P2S5 (i.e., a molar ratio of about 3:1) were dispersed in 50 mL of tetrahydrofuran and stirred at 600 rpm for 24 h at room temperature (25 °C) to obtain a Li3PS4 suspension;
[0077] (2) 0.919 g of Li2S and 0.848 g of LiCl (i.e., a molar ratio of about 2:2) were dissolved in 80 mL of anhydrous ethanol, and then the Li3PS4 suspension was added. After the Li3PS4 suspension was added, the color of the mixed solution changed immediately, and the white precipitate gradually dissolved. After stirring at 600 rpm overnight, the mixed solution was centrifuged at 4000 rpm for 10 min, and the supernatant was collected;
[0078] (3) The collected supernatant was dried under vacuum at 120° C. for 5 h to remove all solvents and obtain a light yellow precursor powder;
[0079] (4) The precursor powder was sintered at 550 °C for 5 h under argon to obtain Li6PS5Cl solid electrolyte.
[0080] Characterization of sulfide solid electrolytes
[0081] XRD characterization: X-ray diffraction (XRD) characterization was performed on the sulfide solid electrolytes prepared in the above Examples 1-3 and Comparative Examples 1-3. Figure 1 As shown, the ordinate is intensity (lntensity) and the abscissa is the diffraction angle (2θ). Figure 1 It can be seen that compared with the comparative example, the XRD spectrum of the embodiment shows that the prepared sulfide solid electrolyte is purer and has less impurities. Among them, compared with Example 1, Example 2 adds an excess of P2S5 to Solution A, which avoids the reaction of Li2S in Solution B with P2S5 to produce other sulfide solid electrolytes, and ensures that the ratio of each raw material does not change when Solution A and Solution B are mixed, thereby obtaining a higher purity Li6PS5Cl solid electrolyte; Example 2 and Example 3 use a specific ratio of raw material components and solvents to prepare sulfide solid electrolytes, and there are almost no raw material impurity peaks such as LiX and Li2S.
[0082] SEM characterization: The sulfide solid electrolyte prepared in Example 2 was subjected to electron microscopy scanning, and its SEM image is as follows: Figure 2 and Figure 3 In addition, it was pressed into a sheet with a diameter of 10 mm and a thickness of 1.6 mm under the conditions of a water content of less than 1 ppm and a pressure of 200 MPa, and the cross section of the pressed sheet was scanned by an electron microscope, and the SEM image was as shown Figure 4 As shown. Figure 2-4 It can be seen that the sulfide solid electrolyte particles prepared in Example 2 of the present invention have a relatively small particle size and do not need to be further refined; after the powder particles are pressed into sheets at a pressure of 200 MPa, the cross section is dense and free of pores.
[0083] Electrochemical performance test of sulfide solid electrolyte
[0084] Under the conditions of water content less than 1ppm and pressure of 200MPa, the sulfide solid electrolytes prepared in Examples 1-3 and Comparative Examples 1-3 were respectively pressed into sheets with a diameter of 10mm and a thickness of 1.6mm. Subsequently, an AC impedance spectrum test was performed at 25°C with a stainless steel sheet as a blocking electrode to evaluate the lithium ion conductivity. The test results are shown in FIG. Figure 5 And as shown in Table 1.
[0085] Table 1
[0086]
[0087] It can be seen from Table 1 that the sulfide solid electrolyte prepared in the embodiment of the present invention has high ion conductivity. At room temperature, the sulfide solid electrolyte exhibits good electrical conductivity, and the lithium ion conductivity of the embodiment is higher than that of the comparative example.
[0088] Compared with Example 1, Comparative Example 1 does not add excessive P2S5 and S, so more ethanol solvent is needed to dissolve Li2S, the side reaction is more serious, resulting in lower lithium ion conductivity; Comparative Examples 2 and Comparative Examples 3 use a solvent or the proportion of raw material components is not within the scope of the present invention, and the lithium ion conductivity is significantly lower.
[0089] In addition, Examples 2 and 3 exhibited high lithium ion conductivity, which was comparable to that of the materials prepared by solid phase ball milling. This indicates that the preparation method of the present invention has significant advantages in preparation purity and efficiency over the traditional liquid phase preparation method, and can be used to quickly prepare Li6PS5X sulfide solid electrolytes with high lithium ion conductivity.
[0090] The preparation method of the present invention can reduce the raw material residue and the formation of Li3PO4 by adjusting the ratio of raw materials and combining different solvents. In addition, the method of preparing the sulfide solid electrolyte by dissolving the elements constituting the solid electrolyte into a specific solvent is simple, fast, efficient and can be mass-produced.
[0091] The preferred embodiments of the present invention are specifically described above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for preparing a sulfide solid electrolyte, characterized in that: The following steps are involved: Mix Li2S, P2S5 and solvent A and stir once to obtain solution A; Mix Li2S, LiX and solvent B, then add elemental sulfur or add elemental sulfur and P2S5, and stir for a second time to obtain solution B, wherein X is selected from Cl, Br or I; The solution B is added to the solution A and stirred three times to obtain a Li-PSX homogeneous solution; The Li-PSX homogeneous solution is dried to remove solvent A and solvent B to obtain a precursor powder; calcining the precursor powder under inert gas conditions to obtain the sulfide solid electrolyte; In the solution A, the molar ratio of Li2S to P2S5 is 1:(1-1.5); In the Li-PSX homogeneous solution, the molar ratio of Li2S, P2S5 and LiX is 5:(1.05-1.5):
2.
2. The preparation method according to claim 1, characterized in that: In the solution B, the molar ratio of Li2S to LiX is (3.5-4.5):
2.
3. The preparation method according to claim 1, characterized in that: In the Li-PSX homogeneous solution, the molar ratio of Li2S, P2S5, LiX and elemental sulfur is 5:(1.05-1.5):2:(0.5-2.5).
4. The preparation method according to claim 1, characterized in that: The solvent A is a polar aprotic solvent, and the solvent A includes at least one of acetonitrile, tetrahydrofuran, tetrahydropyrrole, ethylenediamine, dimethylamine and dimethylformamide.
5. The preparation method according to claim 1, characterized in that: The solvent B is an organic solvent containing a hydroxyl group or a mercapto group, and the solvent B includes at least one of methanol, ethanol, isopropanol, ethanethiol and ethanedithiol.
6. The preparation method according to claim 1, characterized in that: The time of the first stirring is 0.5 to 3 hours; the time of the second stirring is 0.5 to 2 hours; and the time of the third stirring is 0.5 to 4 hours.
7. The preparation method according to claim 1, characterized in that: The drying temperature is 60 to 180° C.; and / or the drying time is 3 to 12 hours.
8. The preparation method according to claim 1, characterized in that: The calcination temperature is 300-600° C.; and / or the calcination time is 2-12 hours.
9. A sulfide solid electrolyte, characterized in that: The sulfide solid electrolyte is prepared by the preparation method according to any one of claims 1 to 8.
10. A solid-state battery, characterized in that: The solid-state battery comprises the sulfide solid-state electrolyte according to claim 9.
Citation Information
Patent Citations
Sulfide solid electrolyte and preparation method and application thereof
CN116072962A
Preparation method of sulfide solid electrolyte
CN118054068A
Method of producing LGPS-based solid electrolyte
JP2021118029A
Slide sleeve hanger system
KR102311309B1
Solid electrolyte material synthesis method
WO2020153973A1
Cited By
Solid electrolyte refining method based on hydrogen bond self-assembly composite aprotic solvent and application of solid electrolyte refining method
CN119965375A
A method for refining a solid electrolyte based on hydrogen bond self-assembly composite aprotic solvent and its application
CN119965375B
Sulfide solid electrolyte, preparation method thereof, battery and application
CN120767395A
Sulfide solid electrolyte and preparation method thereof, battery and application
CN120767395B