Preparation method and application of electroactive polypyrrole bacterial cellulose and platelet-rich plasma bi-crosslinked hydrogel
The preparation of electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel solves the problems of poor mechanical properties and rapid release of growth factors in diabetic ulcer dressings, achieving more effective diabetic wound healing, especially in It has shown good therapeutic effect in type I diabetes mouse model.
Patent Information
- Application Number
- CN202410776466.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
AI Technical Summary
Diabetic ulcers are difficult to heal. The existing dressings have poor mechanical properties. The platelet-rich plasma gel is easy to break. Growth factors are released too quickly and are easily degraded by metal-based proteases in diabetic wounds, resulting in poor therapeutic effects.
The preparation method of electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel is used to form a double cross-linked hydrogel through the cationic polymerization reaction of bacterial cellulose and pyrrole monomers, combined with platelet-rich plasma, which has good Mechanical properties and electrical conductivity to promote wound healing.
The dressing has better mechanical properties and electrical conductivity, can transmit the wound electric field, delay the release of growth factors, and improve the healing effect of diabetic wounds. It especially shows good therapeutic effects on type I diabetes mouse models.
Smart Images

Figure CN118718079A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wound dressing preparation, and in particular to a preparation method and application of an electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel. Background Art
[0002] Diabetic ulcers are an important type of serious and difficult-to-heal skin injury. According to statistics, about 320 million people suffer from diabetes each year, of which about 14% will develop diabetic ulcers. Diabetic ulcers are different from normal skin injuries. They show persistent high-activity inflammatory response and oxidative stress, blocked angiogenesis, and slow proliferation and migration of fibroblasts. The local high blood sugar environment at the diabetic wound is also prone to secondary bacterial infection, resulting in continuous expansion of the ulcer surface and even the final consequence of amputation. Diabetic wound care has always been a huge challenge for skin injury care. Common clinical wound care methods such as wound debridement, negative pressure therapy, and gel dressing treatment can only partially alleviate the disease, and the treatment effect on diabetic ulcers is not satisfactory. In recent years, many excellent treatment methods for diabetic wounds have been developed, such as bioactive dressing therapy, electrical stimulation therapy, photothermal therapy, autologous stem cell sheet therapy, etc., which provide new hope for healing diabetic wounds. Among them, bioactive dressing therapy is a very promising treatment method. Bioactive dressings such as platelet-rich plasma gel are taken from patients. The platelet-rich plasma is purified by centrifugation from autologous plasma and then prepared through a procoagulant reaction; platelet-rich plasma gel has a fibrin skeleton and has good biocompatibility. The large amount of cytokines and growth factors released after platelet degranulation are highly consistent with the growth factors required for the wound healing process, making it a good bioactive dressing for promoting wound healing; however, platelet-rich plasma gel has poor mechanical properties and is easy to rupture and inconvenient to use. The fibrin skeleton is easily degraded by the high concentration of metalloproteinases in diabetic wounds, resulting in the release of large amounts of growth factors in a short period of time, which is not conducive to the treatment of diabetic wounds. Summary of the invention
[0003] The purpose of the present invention is to solve the above problems and to design a preparation method and application of an electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel.
[0004] The present invention provides a preparation method and application of an electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel. The preparation method of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel comprises the following steps:
[0005] Step 1: placing bacterial cellulose hydrogel in a solution containing pyrrole monomers, and adding a solution of ferric chloride to initiate a cationic polymerization reaction of the pyrrole monomers on the bacterial cellulose hydrogel fibers, thereby preparing an electroactive polypyrrole bacterial cellulose hydrogel;
[0006] Step 2: washing the electroactive polypyrrole bacterial cellulose hydrogel prepared in step 1, freezing it in a refrigerator, and then freeze-drying it in a freeze drying box;
[0007] Step 3: Soak the freeze-dried electroactive polypyrrole bacterial cellulose hydrogel in a platelet-rich plasma solution, fully absorb the platelet-rich plasma solution to swell, and then add Ca 2+ The solution promoted the formation of cellulose protein network and platelet degranulation to release growth factors, and obtained electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel.
[0008] Optionally, in the first implementation of the present invention, in step 1, p-toluenesulfonic acid is added as a soft template and a dopant, and the molar ratio of the p-toluenesulfonic acid to the pyrrole monomer is 1:1.
[0009] Optionally, in a second implementation of the present invention, in step 1, the molar ratio of the pyrrole monomer to the ferric chloride is 1:2.26.
[0010] Optionally, in a third implementation of the present invention, the reaction temperature in step 1 is 0°C, and the reaction time is 30 min-2 h.
[0011] Optionally, in a fourth implementation of the present invention, in step 2, after washing, the electroactive polypyrrole bacterial cellulose hydrogel is first cooled with liquid nitrogen and then placed in a -80°C refrigerator for freezing.
[0012] Optionally, in a fifth implementation of the present invention, in step three, the platelet-rich plasma solution is stored at 4°C, and the temperature of the electroactive polypyrrole bacterial cellulose hydrogel during immersion in the platelet-rich plasma solution is 4°C.
[0013] Optionally, in a sixth implementation of the present invention, in step 3, the added Ca 2+ The ratio of platelet-rich plasma solution is 1mL platelet-rich plasma solution plus 50uL of 0.5M Ca 2+ Solution.
[0014] Optionally, in a seventh implementation of the present invention, in step 3, Ca is added 2+ The reaction system was placed at 37°C for 1 hour to promote the formation of the cellulose protein network.
[0015] Optionally, in an eighth implementation of the present invention, in step three, Ca 2+ The solution is calcium chloride solution or calcium gluconate solution.
[0016] Optionally, in a ninth implementation of the present invention, the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel is a diabetic wound dressing.
[0017] The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel provided by the present invention have at least the following beneficial effects compared with the prior art:
[0018] 1. The good mechanical properties of the bacterial cellulose gel used in the present invention make the dressing not easily damaged, and can fit tightly to the wound, reducing the adverse stimulation to the wound;
[0019] 2. The platelet-rich plasma used in the present invention contains a large amount of growth factors, cytokines and microRNAs, and the double network structure can protect against the effects of proteases, etc.;
[0020] 3. The polypyrrole used in the present invention has good electrical conductivity, can transmit the wound injury electric field, guide the fibroblasts to migrate and proliferate to the wound, and thus promote wound healing;
[0021] 4. The present invention has a good sustained-release effect on growth factors loaded in platelet-rich plasma. The release curves of platelet-derived growth factor, transforming growth factor β, and vascular endothelial growth factor show that the double-crosslinked hydrogel of the present invention has a more durable and stable growth factor release capacity;
[0022] 5. The present invention has a good promoting effect on diabetic wound healing and has a good therapeutic effect on the wound model of type I diabetic mice;
[0023] 6. The dressing prepared by the present invention combined with exogenous electrical stimulation can controllably regulate the release of growth factors and provide low-voltage electrical stimulation to the wound, further promoting wound healing. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the following detailed description of the preferred embodiment.The drawings are only for the purpose of illustrating the preferred embodiments and are not to be construed as limiting the invention.
[0025] Figure 1 It is a schematic diagram of the preparation method of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel provided by the present invention;
[0026] Figure 2These are light microscopic and electron microscopic photographs of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double-crosslinked hydrogel wound dressing provided by the present invention;
[0027] Figure 3 This is a test diagram of the mechanical properties of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel provided by the present invention;
[0028] Figure 4 This is a test diagram of the electrical conductivity of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel provided by the present invention;
[0029] Figure 5 The release curve of platelet plasma growth factor, transforming growth factor β and vascular endothelial growth factor over time in the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel provided by the present invention;
[0030] Figure 6 This is a diagram of the wound repair of type I diabetic mice using the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel wound dressing provided by the present invention. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Bacterial cellulose gel has a wide range of applications in the field of skin injuries. It has good mechanical properties, high water absorption, and high water retention, which is conducive to absorbing inflammatory exudates from wounds and maintaining a moist healing environment for wounds. By combining bacterial cellulose gel with platelet-rich plasma gel, bacterial cellulose / platelet-rich plasma double-crosslinked hydrogel is prepared, thereby overcoming the problem that platelet-rich plasma gel is easy to break and inconvenient to use. The rich fiber network of bacterial cellulose can also play a sustained-release role for cytokines and growth factors stored in platelet-rich plasma, solving the problem of too fast growth factor release in platelet-rich plasma gel; in addition, electrical signals are important physical signals in the wound healing process, and the skin injury electric field plays an important role in guiding fibroblasts to migrate, attach and proliferate to the wound. Studies have found that electrical stimulation can also promote blood perfusion of the wound, promote wound microvascular regeneration, and regulate the wound. The oral immune microenvironment plays an important role in wound healing. Electroactive wound dressings can promote the transmission of electrical stimulation at the wound site, thereby promoting the migration and colonization of damage repair-related cells to the wound site, and promoting the healing of difficult-to-heal wounds such as diabetic ulcers. Therefore, adding electroactive substances such as polypyrrole to bacterial cellulose / platelet-rich plasma double cross-linked hydrogels to prepare electroactive bacterial cellulose / platelet-rich plasma wound dressings can not only enhance the repair effect of the dressing on diabetic ulcers, but also regulate the release rate of growth factors in platelet-rich plasma through low-voltage electrical stimulation to achieve the purpose of controlled sustained release, thereby providing a refined and effective wound care solution for the treatment of diabetic ulcers.
[0033] See also Figure 1 The present invention provides a method for preparing an electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel, and the preparation method specifically comprises the following steps:
[0034] Step 1: placing bacterial cellulose hydrogel in a solution containing pyrrole monomers, and adding a solution of ferric chloride to initiate a cationic polymerization reaction of the pyrrole monomers on the bacterial cellulose hydrogel fibers, thereby preparing an electroactive polypyrrole bacterial cellulose hydrogel;
[0035] In this step, p-toluenesulfonic acid is added as a soft template and dopant, and the molar ratio of p-toluenesulfonic acid to pyrrole monomer is 1:1; the molar ratio of pyrrole monomer to ferric chloride is 1:2.26; the reaction temperature of this step is 0°C, and the reaction time is 30min-2h.
[0036] In this step, bacterial cellulose is obtained by static culture secretion of xylinum acetobacter, a fermentation medium of xylinum acetobacter is prepared, and xylinum acetobacter is cultured in the fermentation medium. The medium is statically cultured in a biochemical incubator for one week, and a layer of bacterial cellulose hydrogel film is formed on the surface of the medium. The bacterial cellulose hydrogel film is taken out, washed twice with a sodium hydroxide solution, and then washed three times by boiling with ultrapure water to obtain a purified bacterial cellulose hydrogel; polypyrrole is prepared by an in-situ cationic polymerization reaction of a pyrrole monomer, and the bacterial cellulose hydrogel is cut and placed in an aqueous solution containing a pyrrole monomer and p-toluenesulfonic acid, and then placed in an ice-water mixed bath for stirring. A bottle of aqueous solution containing ferric chloride is also prepared, and the ferric chloride solution is poured into the above reaction solution, and the mixture is rapidly stirred and timing is started. After a period of reaction, the pure white bacterial cellulose hydrogel can be seen to be gradually covered by black polypyrrole, and then the prepared polypyrrole bacterial cellulose hydrogel is taken out, washed three times by ultrasonic oscillation, and soaked overnight. The purified polypyrrole bacterial cellulose hydrogel is placed in a refrigerator for freezing, and then placed in a freeze drying box for freeze drying to obtain a freeze-dried polypyrrole bacterial cellulose gel.
[0037] Step 2: washing the electroactive polypyrrole bacterial cellulose hydrogel prepared in step 1, freezing it in a refrigerator, and then freeze-drying it in a freeze drying box;
[0038] In this step, after washing, the electroactive polypyrrole bacterial cellulose hydrogel is first cooled with liquid nitrogen and then placed in a -80°C refrigerator for freezing; the platelet-rich plasma solution is stored at 4°C, and the temperature of the electroactive polypyrrole bacterial cellulose hydrogel during immersion in the platelet-rich plasma solution is 4°C.
[0039] Step 3: Soak the freeze-dried electroactive polypyrrole bacterial cellulose hydrogel in a platelet-rich plasma solution, fully absorb the platelet-rich plasma solution to swell, and then add Ca 2+ The solution promoted the formation of cellulose protein network and platelet degranulation to release growth factors, and obtained electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel.
[0040] In this step, Ca 2+ The solution is a calcium chloride solution or a calcium gluconate solution, and the ratio of the added calcium chloride solution or calcium gluconate solution to the platelet-rich plasma solution is 1 mL of the platelet-rich plasma solution plus 50 uL of a 0.5 M calcium chloride solution or calcium gluconate solution; after adding the calcium chloride solution or calcium gluconate solution, the reaction system is placed at 37° C. for 1 hour to promote the formation of a cellulose protein network.
[0041] In this step, Ca 2+Activated platelet degranulation releases a large amount of growth factors and cytokines loaded in the double network hydrogel. Due to the sustained release effect of the double network hydrogel, when used as a wound dressing (diabetic wound dressing), the growth factors in the platelet-rich plasma can slowly and continuously act on the wound (diabetic wound), promote the vascularization of the wound (diabetic wound), and inhibit the inflammatory response. The electroactive polypyrrole can also transmit the wound damage electric field, combined with exogenous electrical stimulation, to promote the migration and proliferation of fibroblasts and endothelial cells to the wound, thereby promoting wound healing.
[0042] In this step, platelet-rich plasma is prepared by centrifugation of autologous whole blood or whole blood from donors of the same blood type.
[0043] In this step, the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel is a diabetic wound dressing; since polypyrrole is a conductive polymer, the bacterial cellulose fiber modified with polypyrrole can provide a good conduction path for the damage electric field at the wound, and guide the cells to migrate along the electric field; since the growth factors released from the platelet-rich plasma are wrapped by the cellulose protein network and the bacterial cellulose network, the release of the growth factors in the platelet-rich plasma is slowed down, providing a continuous growth factor concentration for diabetic wound healing; the bacterial cellulose has good mechanical properties, so that the dressing is not easy to break during use and is easy to use; the polypyrrole bacterial cellulose dressing is electrically responsive, and the network structure of the hydrogel can be adjusted under an external electric field, thereby achieving the purpose of regulating the release of growth factors in platelet-rich plasma.
[0044] The preparation method of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel is described in detail below in conjunction with specific preferred embodiments.
[0045] Embodiment 1:
[0046] 1. Preparation of bacterial cellulose hydrogel:
[0047] Step S11: preparing a fermentation medium for Gluconacetobacter xylinum: 15 g / L glucose, 10 g / L peptone, 5 g / L yeast extract, 2 g / L sodium dihydrogen phosphate, and 2 g / L disodium hydrogen phosphate;
[0048] Step S12: Gluconacetobacter xylinum is cultured in the fermentation medium of step S11, and cultured in a biochemical incubator at 30° C. for one week, and a layer of bacterial cellulose hydrogel film is formed on the surface of the culture medium;
[0049] Step S13: taking out the bacterial cellulose hydrogel membrane, washing it twice with a 0.1 M sodium hydroxide solution, and then washing it three times with boiling ultrapure water to obtain a purified bacterial cellulose hydrogel.
[0050] 2. Preparation of electroactive polypyrrole bacterial cellulose hydrogel:
[0051] Step S21: Cut the bacterial cellulose hydrogel, place it in 95 mL of an aqueous solution containing 0.20 g of pyrrole monomer and 0.51 g of p-toluenesulfonic acid, and place it in a 0° C. ice-water mixing bath and stir;
[0052] Step S22: Prepare another 5 mL bottle of aqueous solution containing 1.09 g of ferric chloride, pour the ferric chloride solution into the above reaction solution, stir rapidly and start timing;
[0053] Step S23: After reacting for 1 hour, it can be seen that the pure white bacterial cellulose hydrogel is gradually covered by black polypyrrole, and then the prepared polypyrrole bacterial cellulose hydrogel is taken out, washed three times by ultrasonic oscillation, and soaked overnight;
[0054] Step S24: The purified polypyrrole bacterial cellulose hydrogel is placed in a -80°C refrigerator for 12 hours, and then placed in a freeze drying box for lyophilization for 48 hours to obtain a lyophilized polypyrrole bacterial cellulose gel.
[0055] 3. Preparation of electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel:
[0056] Step S31: a platelet-rich plasma solution is obtained by centrifuging whole blood. Blood is collected from a vein aseptically and quickly placed in an EDTA anticoagulant tube. The whole blood is centrifuged at a low speed of 1000 rpm for 5 minutes in a refrigerated centrifuge to obtain the upper layer solution. The whole blood is then centrifuged at a high speed of 5000 rpm for 15 minutes to obtain the bottom two layers of the platelet-rich plasma solution.
[0057] Step S32: cutting the freeze-dried polypyrrole bacterial cellulose into a suitable size, placing it in the platelet-rich plasma solution, and soaking it at 4° C. with shaking overnight to allow it to fully re-swell;
[0058] Step S33: taking out the re-swollen polypyrrole bacterial cellulose / platelet-rich plasma, adding calcium chloride or calcium gluconate solution at a ratio of platelet-rich plasma solution: 0.5M calcium chloride solution = 10:1, and placing at 37°C to stand to form gel;
[0059] Step S34: The prepared electroactive polypyrrole bacterial cellulose / platelet-rich plasma hydrogel is stored in a refrigerator at 4°C for 1 week, or can be stored for a long time after freeze-drying. The digital photo and electron microscope photo of the prepared electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel are as follows: Figure 2 shown.
[0060] Embodiment 2:
[0061] Mechanical properties test of electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel:
[0062] The electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel prepared in Example 1 was cut into dumbbell shapes with 5 cm*2 cm at both ends and 2 cm*2 cm in the middle, and clamped on a universal tensile tester; the thickness of the polypyrrole bacterial cellulose / platelet-rich plasma hydrogel was measured, and the tensile speed of the universal tensile tester was set to 10 mm / min. The stress-strain curve of the hydrogel was drawn by judging that 80% stress decay was the breaking point, as shown in FIG. Figure 3 shown.
[0063] Embodiment 3:
[0064] Conductive properties of electroactive polypyrrole bacterial cellulose / platelet-rich plasma hydrogels were tested, such as Figure 4 As shown:
[0065] The electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel prepared in Example 1 was spread on an insulating board, and a four-probe resistance tester was pressed on the surface of the material with a constant force, and the current value I flowing through probes 1 and 4 and the voltage value V measured by probes 2 and 3 were recorded, and the surface resistance of the material was calculated by R=V / I*Fsp;
[0066] The electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel prepared in Example 1 was placed on the working electrode of the electrochemical workstation, with a platinum sheet electrode as the working electrode, a saturated amalgam electrode SCE as the reference electrode, a 0.9% sodium chloride solution as the electrolyte solution, a voltage window of -1V-1V, and a scan rate of 20mV / s to record the voltammetric characteristic curve of the material.
[0067] Embodiment 4:
[0068] Release of growth factors from electroactive polypyrrole bacterial cellulose / platelet-rich plasma hydrogels, e.g. Figure 5 As shown:
[0069] The electroactive polypyrrole bacterial cellulose / platelet-rich plasma double cross-linked hydrogel and pure platelet-rich plasma hydrogel prepared in Example 1 were placed in a 6-well plate, 5 mL of phosphate buffer was added to each well of the 6-well plate, and the plates were placed in a 37° C., 5% CO2 cell culture incubator for different incubation times;
[0070] At 30 minutes, 1 hour, 4 hours, 1 day, 2 days, 3 days, 4 days, 5 days, 6 days, and 7 days, 0.5 mL of liquid was removed from the sample and 0.5 mL of fresh phosphate buffer was added. The removed liquid was stored in a refrigerator at -80 °C for future use;
[0071] The absorbance of the solution obtained at each time point was tested by enzyme-linked immunofluorescence labeling and compared with the standard curve to obtain the release curve of different growth factors over time.
[0072] Embodiment 5:
[0073] Electroactive polypyrrole bacterial cellulose / platelet-rich plasma hydrogel for the treatment of diabetic wounds in mice:
[0074] 40 healthy adult male BABL / c mice weighing 20g-22g were selected. After fasting for 12 hours, they received a single intraperitoneal injection of streptozotocin (STZ) (50mg / kg) to induce type I diabetes. Three days after induction, blood was collected from the tail vein and tested using a blood glucose meter kit. The blood glucose level of diabetic mice after STZ injection was higher than 14mmol / L, indicating that the model was successfully established;
[0075] After successful induction of type 1 diabetes, mice were anesthetized with 0.3% sodium pentobarbital injected intraperitoneally, and excess hair was removed with an electric shaver. After disinfection with povidone solution, a 10 mm full-thickness skin injury was made on the back of the mice using a sterile skin burr.
[0076] All mice were randomly divided into four groups: the control group was treated with commercial 3M dressing, the PRP group was treated with pure platelet-rich plasma hydrogel, the PBP group was treated with electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel, and the PBP+EF group was treated with electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel and exogenous direct current stimulation (DC=1V) for 1 hour per day;
[0077] Wounds were macroscopically examined on days 0, 3, 7, 10, and 14, and wound recovery was estimated by photographing the wounds with a digital camera, and wound size was calculated to assess wound healing rate, e.g. Figure 6 shown.
[0078] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. Preparation method and application of electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel, characterized in that: The preparation method of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel comprises the following steps: Step 1: placing bacterial cellulose hydrogel in a solution containing pyrrole monomers, and adding a solution of ferric chloride to initiate a cationic polymerization reaction of the pyrrole monomers on the bacterial cellulose hydrogel fibers, thereby preparing an electroactive polypyrrole bacterial cellulose hydrogel; Step 2: washing the electroactive polypyrrole bacterial cellulose hydrogel prepared in step 1, freezing it in a refrigerator, and then freeze-drying it in a freeze drying box; Step 3: Soak the freeze-dried electroactive polypyrrole bacterial cellulose hydrogel in a platelet-rich plasma solution, fully absorb the platelet-rich plasma solution to swell, and then add Ca 2+ The solution promoted the formation of cellulose protein network and platelet degranulation to release growth factors, and obtained electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel.
2. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step one, p-toluenesulfonic acid is added as a soft template and a dopant, and the molar ratio of the p-toluenesulfonic acid to the pyrrole monomer is 1:
1.
3. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step 1, the molar ratio of the pyrrole monomer to the ferric chloride is 1:2.
26.
4. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: The reaction temperature of step 1 is 0°C, and the reaction time is 30min-2h.
5. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step 2, after washing, the electroactive polypyrrole bacterial cellulose hydrogel is first cooled with liquid nitrogen and then placed in a -80°C refrigerator for freezing.
6. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step three, the platelet-rich plasma solution is stored at 4° C., and the temperature of the electroactive polypyrrole bacterial cellulose hydrogel is 4° C. during the period in which the electroactive polypyrrole bacterial cellulose hydrogel is immersed in the platelet-rich plasma solution.
7. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step 3, the Ca 2+ The ratio of platelet-rich plasma solution is 1mL platelet-rich plasma solution plus 50uL of 0.5M Ca 2+ Solution.
8. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step 3, add Ca 2+ The reaction system was placed at 37°C for 1 hour to promote the formation of the cellulose protein network.
9. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: In step 3, Ca 2+ The solution is calcium chloride solution or calcium gluconate solution.
10. The preparation method and application of the electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel according to claim 1, characterized in that: The electroactive polypyrrole bacterial cellulose and platelet-rich plasma double cross-linked hydrogel is a diabetic wound dressing.
Citation Information
Cited By
Bionic hydrogel for treating cartilage defect and preparation method thereof
CN121401481A