Pectin microspheres capable of rapidly stopping bleeding and promoting wound healing and preparation method of pectin microspheres

Pectin microspheres prepared by emulsification cross-linking method, combined with acellular skin matrix and divalent cations, form multifunctional pectin microspheres, which solves the problems of poor wound healing, hemostasis and antibacterial effects in the existing technology. It achieves rapid hemostasis, antibacterial and wound healing effects, and has good biological safety.

CN118718103APending Publication Date: 2024-10-01CHONGQING UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410717654.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology lacks multifunctional materials in terms of promoting wound healing, rapid hemostasis and antibacterial, and has uncontrollability and biosafety issues.

Method used

It uses pectin microspheres prepared from acellular skin matrix, pectin and divalent cations through emulsification and cross-linking methods to form microspheres with a three-dimensional network structure. It combines natural bioactive factors and cellulose to provide wound healing and Multifunctional material to stop bleeding.

Benefits of technology

It achieves the multi-functional effects of rapid hemostasis, antibacterial, anti-inflammatory and wound healing promotion. It also has good biosafety and low toxicity and is suitable for hemostatic agents and wound dressings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004876034220000051
    Figure BDA0004876034220000051
  • Figure HDA0004876034230000011
    Figure HDA0004876034230000011
  • Figure HDA0004876034230000012
    Figure HDA0004876034230000012
Patent Text Reader

Abstract

The invention discloses pectin microspheres capable of rapidly stopping bleeding and promoting wound healing and a preparation method of the pectin microspheres. The microspheres are prepared from an acellular skin matrix, pectin and divalent cations through an emulsification cross-linking method. The pectin microspheres prepared by the invention not only have a three-dimensional porous structure similar to natural skin, but also can provide a microenvironment closest to the nature for tissue repair under the condition of not causing immunological rejection, are beneficial to adhesion and growth of cells, are also beneficial to proliferation and differentiation of dermal fibroblasts, keratinocytes and the like, and have a good application prospect. The repair and regeneration of skin tissues can be promoted. The pectin microspheres provided by the invention realize multifunctional application of rapid hemostasis, antibiosis and promotion of wound healing, have good biological safety, are a very safe and easily available biological material, and have wide application prospects in hemostasis and skin repair promotion engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tissue engineering materials, and in particular to pectin microspheres capable of rapidly stopping bleeding and promoting wound healing, and a preparation method thereof. Background Art

[0002] As the largest organ in the human body, the skin is the easiest and most frequently injured. Once the skin is damaged, it undergoes a dynamic and complex healing process - hemostasis, inflammation, proliferation and remodeling. Interruptions or abnormalities in this process may lead to delayed wound healing or chronic wound non-healing. Long hemostasis time and delayed healing will increase the risk of wound infection, leading to repeated wounds and even scarring. Therefore, rapid hemostasis and promotion of wound healing can help increase the skin healing rate and improve the healing effect.

[0003] At present, research on promoting wound healing mainly focuses on the expression and functional role of growth factors in skin wound repair. The main treatment methods include combining recombinant growth factors and living cells, local delivery of growth factors, stem cell therapy and regulating the wound microenvironment. For example, the invention patent CN114073759A discloses a skin wound healing preparation, wherein the active ingredients of the skin wound healing preparation include epidermal growth factor and / or fibroblast growth factor. By combining growth factors in dressings, skin repair is promoted by releasing growth factors, but the expression and growth-promoting effect of growth factors in this method are uncontrollable. The invention patent CN117482280A discloses a method for preparing a blood cell active hydrogel for wound repair, which gives the hydrogel photoresponsiveness by adding black phosphorus quantum dots, so that the red blood cells on the hydrogel can controllably release oxygen under near-infrared light irradiation. This method is to indirectly promote wound healing by regulating the microenvironment with hydrogels, adding oxygen supply, anti-inflammatory and sterilization functions, but the healing method of hydrogel oxygen supply and sterilization requires controlling the dosage of oxygen release agents, and the raw materials may be cytotoxic. Skin regeneration and repair are also promoted by inducing stem cell differentiation, but the gene therapy process is often accompanied by inflammation. Therefore, these existing methods have defects in practice. At the same time, rapid hemostasis and antibacterial effects can effectively prevent secondary wound damage, promote wound healing, and reduce traumatic complications. However, in the prior art, there are few reports of materials that have multiple functions such as promoting wound healing, rapid hemostasis, and antibacterial. Therefore, how to develop a multifunctional application with rapid hemostasis, antibacterial, and promotion of wound healing, and good biosafety, is of great value to surgical hemostasis.

[0004] Decellularized matrix is ​​a potential material that has attracted widespread attention in the field of tissue engineering due to its good biocompatibility, degradability, extremely low toxicity and low immunogenicity. It removes immunogenicity and retains the spatial structure of ECM and a large number of extracellular signaling molecules. It has almost the same biochemical composition and structure as natural tissue. The most critical thing is that the bioactive factors it contains play an important role in regulating cell behavior. The extracellular matrix from different tissues provides a specific tissue microenvironment for cell-directed mitosis, differentiation, apoptosis, differential adhesion and morphogenesis. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a pectin microsphere having the functions of rapid hemostasis and promoting wound healing and a preparation method thereof, so as to solve the problems of the prior art such as uncontrollable, slow healing and lack of multifunctional properties.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solution: a pectin microsphere with both rapid hemostasis and wound healing, wherein the microsphere is prepared by emulsification cross-linking of decellularized skin matrix, pectin and divalent cations. In this way, the cross-linking of low-fat pectin mainly depends on the fact that the carboxyl groups present in large quantities in pectin can be cross-linked with divalent cations such as calcium and magnesium, and the formed gel usually has a three-dimensional water-insoluble network structure that can adsorb and fix water or other substances. The decellularized matrix solution is evenly mixed in the network structure, but because it also contains a certain amount of carboxyl groups, it participates in the cross-linking to a greater or lesser extent.

[0007] Preferably, the particle size of the microspheres is 10 to 100 μm.

[0008] Preferably, the divalent cations include but are not limited to Ca 2+ Mg 2+ 、Zn 2+ , Cu 2+ or Mn 2+ wait.

[0009] Another object of the present invention is to provide a method for preparing the above-mentioned pectin microspheres having both rapid hemostasis and wound healing properties, comprising the following steps:

[0010] 1) dissolving pectin in water to prepare a pectin solution with a mass concentration of 1 to 4%, and then mixing the prepared acellular skin matrix solution and the pectin solution to obtain a matrix-pectin mixed solution for later use;

[0011] 2) placing the oil phase in a water bath at 40-45° C., adding an emulsifier, stirring evenly, then dropping the matrix-pectin mixed solution obtained in step 1), maintaining the same temperature and speed, continuing stirring, then adding a cross-linking agent containing divalent cations, maintaining the same temperature and speed, continuing stirring, and obtaining a reaction product after the reaction is completed;

[0012] 3) The reaction product obtained in step 2) is washed with petroleum ether and anhydrous ethanol for multiple times, and freeze-dried to obtain the pectin microspheres.

[0013] Preferably, the acellular skin matrix solution is prepared by the following steps: taking animal dermal tissue, removing excess impurities and cutting into small pieces, removing subcutaneous fat and cleaning, and then soaking in a 0.25% trypsin solution for 12 hours, in 70% isopropanol containing 0.1% SDS for 12 hours, in 70% isopropanol containing 1% Triton X-100 for 12 hours, and in 100% isopropanol for 12 hours at 37°C, and then shaking and washing with a large amount of deionized water, freeze-drying, and then digesting the freeze-dried tissue with pepsin under acidic conditions. After the reaction is completed, centrifugation is performed to remove cell debris and other impurities to obtain a decellularized dermal matrix solution.

[0014] Preferably, the mass concentration ratio of the decellularized skin matrix to pectin in the mixed solution is 1:10-40; and the pH value of the decellularized skin matrix solution is 7.0-7.5.

[0015] Preferably, the oil phase is liquid paraffin or vegetable oil; the emulsifier is one or more of Span80 and Tween20; and the amount of the emulsifier added is 1% to 10% of the volume of the oil phase.

[0016] Preferably, the cross-linking agent containing divalent cations is calcium chloride, magnesium chloride or zinc chloride, etc. The mass concentration of divalent cations in the cross-linking agent is 2-10%.

[0017] Preferably, the stirring speed in step 2) is 500-1000 rpm.

[0018] Another object of the present invention is to provide the use of the pectin microspheres prepared by the above method in the preparation of drugs related to hemostasis and skin repair, such as but not limited to wound dressings, hemostatic agents and drug delivery carriers.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The matrix-pectin microspheres prepared by the present invention are a composite of pectin and acellular skin matrix, and then cross-linked with divalent cations to form a microscopic three-dimensional structure. The added acellular matrix removes the cellular components in the tissue, so that the obtained pectin microspheres not only have a three-dimensional porous structure similar to natural skin, but also contain natural fiber components such as collagen fibers and a variety of cell growth factors, etc., which can provide the closest natural microenvironment for tissue repair without causing immune rejection, which is conducive to the adhesion and growth of cells, and is also conducive to the proliferation and differentiation of dermal fibroblasts, keratinocytes, etc., and can promote the repair and regeneration of skin tissue. At the same time, the unique porous structure of pectin materials and microspheres can promote hemostasis to a certain extent. Finally, the pectin material itself also has anti-inflammatory and antioxidant effects, can scavenge free radicals, inhibit the release of inflammatory mediators, thereby reducing the occurrence of oxidative stress; and the presence of cellulose helps to form a protective dressing on the wound, thereby preventing infection and promoting wound healing. Therefore, the present invention realizes the multifunctional application of rapid hemostasis, antibacterial and anti-inflammatory, and promotion of wound healing, and has good biological safety.

[0021] 2. The present invention uses pectin and acellular matrix as raw materials, both of which are natural biological materials, and have many advantages such as low price, good biocompatibility, and biodegradability. The preparation method is simple, and the obtained pectin microspheres have a compact porous structure, which can stop bleeding, have antibacterial and anti-inflammatory effects, and promote wound healing. Therefore, this is a very safe and easily available biomaterial, and has broad application prospects in hemostasis and skin repair engineering, such as wound dressings, hemostatic agents, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Comparison of HE staining and Masson staining before and after acellular skin matrix.

[0023] Figure 2 For quantitative analysis of DNA before and after acellular skin matrix.

[0024] Figure 3 This is a microscopic morphology of the pectin microspheres prepared in the present invention.

[0025] Figure 4 This is a statistical diagram of the particle size of the pectin microspheres prepared in the present invention.

[0026] Figure 5 This is the infrared spectrum analysis of the pectin microspheres prepared by the present invention.

[0027] Figure 6 This is a swelling rate curve of the pectin microspheres prepared in the present invention.

[0028] Figure 7 This is the hemolysis condition of the pectin microspheres prepared by the present invention.

[0029] Figure 8 It is the hemolysis rate of the pectin microspheres prepared by the present invention.

[0030] Fig. 9 The static coagulation condition and coagulation time of the pectin microspheres prepared in the present invention.

[0031] Fig.10 This is the dynamic coagulation curve of the pectin microspheres prepared in the present invention.

[0032] Fig.11 The microscopic morphology of the pectin microspheres prepared in the present invention adsorbing red blood cells.

[0033] Fig.12 The red blood cell consumption rate and adhesion rate of the pectin microspheres prepared by the present invention. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below with reference to the examples. The reagents used in the examples are commercially available unless otherwise specified.

[0035] Example 1

[0036] A pectin microsphere having the functions of rapid hemostasis and promoting wound healing is prepared by the following method:

[0037] 1) Wash fresh porcine dermis thoroughly with distilled water, remove attached dirt and debris, and cut into 0.5cm×0.5cm square pieces. Remove subcutaneous fat, clean and soak in trypsin solution (0.25%) at 37°C for 12h. Then, keep the same temperature, soak in 70% isopropanol containing 0.1% SDS for 12h, soak in 70% isopropanol containing 1% Triton X-100 for 12h, and finally soak in 100% isopropanol for 12h to remove fat. Then wash the sample thoroughly with distilled water and freeze-dry it with a freeze dryer. Cut the freeze-dried tissue into pieces, add 10mL of 0.5M glacial acetic acid, 100mg of pepsin (1:10000) and 5mg of phosphate buffer powder for digestion per 100mg of tissue. After digestion, centrifuge the digested mixture to remove cell debris and other impurities to obtain acellular dermal matrix fluid, which is stored in a -20°C refrigerator for use. When using acellular dermal matrix, adjust the pH to 7.4 with NaOH in an ice bath to obtain an acellular skin matrix solution in the form of a milky white transparent gel for later use.

[0038] 2) dissolving pectin in water to prepare a pectin solution with a mass concentration of 4%, and then mixing the acellular skin matrix solution prepared in step 1), the pectin solution and water in a volume ratio of 10:4:6 to prepare a matrix-pectin mixed solution with a final mass concentration ratio of matrix to pectin of 1:10 and a pectin concentration of 2%.

[0039] 3) Take 50 mL of liquid paraffin and preheat it in a water bath at 40° C., add 2 mL of Span80, set the magnetic stirrer at 40° C., stir evenly at a speed of 600 rpm, then add 10 mL of the matrix-pectin solution with a syringe, maintain the same temperature and speed, continue stirring for 30 minutes, then add 5 mL of a 10% calcium chloride solution, maintain the same temperature and speed, continue stirring for 1 hour, and obtain the reaction product after the reaction is completed.

[0040] 4) The reaction product obtained in step 3) is washed with petroleum ether and anhydrous ethanol for 2 to 3 times in sequence, and then freeze-dried to obtain the pectin microspheres.

[0041] The operation steps of Examples 2 to 3 and Comparative Examples 1 to 3 are the same as those of Example 1, except that the mass concentrations of pectin and acellular skin matrix in the matrix-pectin mixed solution are different, as shown in Table 1.

[0042] Table 1

[0043]

[0044] 2. Performance Testing

[0045] 1. HE staining and MASSON staining were performed on fresh pig skin before and after decellularization to analyze the decellularization effect. The results are as follows: Figure 1 shown.

[0046] As can be seen from the figure, compared with the control group, the outer color of the pig skin after decellularization becomes white. In HE staining, there are a large number of blue-purple nuclei and pink cytoplasm in fresh pig skin, while almost no blue-purple nuclei can be seen in the sections of decellularized pig skin, only pink cytoplasm. This result shows that the present invention can effectively remove cells in pig skin tissue while retaining its natural extracellular matrix. In MASSON staining, the content of collagen fibers after decellularization does not change much, indicating that after decellularization, the cells are effectively removed while the matrix structure and collagen are retained. Further, the fresh pig skin was subjected to deoxyribonucleic acid (DNA) quantitative analysis before and after decellularization, and the results are as follows. Figure 2 As shown in the figure, it can be seen that most of the deoxyribonucleic acid is removed from the natural tissue after the decellularization treatment. In summary, it is shown that the decellularization process of the present invention is effective.

[0047] 2. The microscopic morphology and particle size statistics of the pectin microspheres prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were observed under an electron microscope. The results are as follows: Figures 3-4 shown.

[0048] As can be seen from the figure, three different concentrations of pectin can form microspheres through emulsification cross-linking, and their particle sizes are all within 100μm. However, as the pectin concentration increases, the particle size of the microspheres gradually decreases, and the uniformity is more dispersed. Among them, when the pectin mass concentration is 2%, the pectin microspheres have a higher particle size uniformity, and more than 60% of the microspheres have a particle size of 40-60μm. Keeping the pectin mass concentration at 2%, and using three different matrix-pectin concentration ratios of mixed solutions (Examples 1-3) can also form microspheres through cross-linking, and the particle size is 0-100μm. However, as the matrix concentration decreases, the microsphere particle size range is more dispersed and the uniformity decreases. Among them, when the matrix to pectin concentration ratio is 1:10, the pectin microspheres have a higher particle size uniformity, and more than 50% of the microspheres have a particle size of 30-50μm.

[0049] 3. The pectin microspheres and the decellularized matrix (ECM) prepared in Examples 1 to 3 and Comparative Example 1 were analyzed by Fourier transform infrared spectrometer from Perkin Elmer, USA. The results are as follows: Figure 5 shown.

[0050] It can be seen from the figure that at a wavelength of 3600cm -1 To 3200cm -1 There are stretching vibration peaks of hydroxyl OH in the places, but the intensity and area of ​​the peaks are different between groups, and there is a certain shift; the wavelength is 2924cm -1 and 2854cm -1 It is the symmetric and antisymmetric stretching vibration peak of CH2; wavelength 1380cm -1 and 1468cm -1 It is the symmetric stretching vibration and antisymmetric stretching vibration peak of carboxylate COO. The peaks of pure pectin microspheres (Comparative Example 1) and matrix-pectin microspheres (Examples 1 to 3) are significantly different from the peaks of pectin powder, indicating that the cross-linking of pectin has occurred chemical bond breakage and recombination, and the cross-linking is successful. Further, the infrared spectra of pure pectin microspheres (Comparative Example 1) and matrix-pectin microspheres (Examples 1 to 3) are basically consistent, but the peak intensity and area are different, indicating that the addition of the matrix leads to the breakage and recombination of chemical bonds, which further leads to changes in content.

[0051] 4. The pectin microspheres prepared in Examples 1 to 3 were tested for swelling properties. Different microspheres were dissolved in PBS solution at the same time, taken out at different time points, and then the surface water was dried and weighed. The results are as follows: Figure 6 shown.

[0052] It can be seen from the figure that the microspheres of Examples 1 to 3 swelled rapidly in the first half an hour and remained basically stable after 2 hours. Among them, the microspheres with a larger matrix-pectin mass concentration ratio had a higher swelling rate, and the microspheres with a smaller mass concentration ratio had a smaller swelling rate.

[0053] 5. Hemolytic experiments were conducted on Examples 1 to 3, and the hemolytic conditions and hemolytic rates of the microspheres were observed and counted. The results are as follows: Figures 7-8 shown.

[0054] As can be seen from the figure, compared with the positive control group, no obvious hemolysis occurred in all samples ( Figure 7 The hemolysis rates of the microspheres of Examples 1 to 3 were 1.766±0.7276%, 2.021±0.9746%, and 2.148±0.8337%, respectively. Figure 8 ), the overall hemolysis rate was less than 5%. According to the national standard GB / T16886.4, the hemolysis degree of the microspheres prepared by the present invention is within the standard range and meets the national safety standards for biomaterials.

[0055] 6. The pectin microspheres prepared in Comparative Example 1 and Examples 1 to 3 were subjected to a static coagulation test, and the coagulation time was recorded and counted. The results are as follows: Fig. 9 shown.

[0056] As can be seen from the figure, the coagulation times of Comparative Example 1 (control group) and Examples 1 to 3 are 8'34"±8", 1'2"±8", 1'32"±5" and 1'54"±4", respectively. Compared with the control group, the coagulation time of the microspheres of the present invention is shorter, and the coagulation time increases with the decrease of the matrix-pectin concentration ratio. This shows that the pectin microspheres of the present invention have the ability to promote coagulation, and the microsphere group with a larger matrix-pectin concentration has a faster coagulation efficiency.

[0057] 7. Dynamic coagulation test was performed on the pectin microspheres prepared in Examples 1 to 3. The results are as follows: Fig.10 shown.

[0058] As can be seen from the figure, with the passage of time, the BCI index of the three groups of different microspheres gradually decreases. At 1 minute, the BCI value of Example 1 is higher than that of Example 2 and higher than that of Example 3, but after 10 minutes, the BCI of the microspheres of Examples 1 to 3 are 38.802±4.241%, 43.224±2.159% and 39.693±5.104%, respectively, and there is no significant difference among the three groups. This shows that the three groups of microspheres have a certain effect of promoting coagulation, and at the beginning of hemostasis, the microspheres with a larger matrix-pectin concentration ratio can promote hemostasis faster. After a period of time, the overall coagulation ability of each group of microspheres is similar.

[0059] 8. The red blood cell consumption rate and adhesion rate of the pectin microspheres prepared in Examples 1 to 3 were tested by calculating the blood cell concentration of the supernatant. The group without microspheres was used as the blank control group. The results are as follows: Figures 11-12 shown.

[0060] It can be seen from the figure that the microsphere surfaces of Examples 1 to 3 can adsorb a considerable number of red blood cells ( Fig.11 ), the red blood cell adsorption amount of Example 1 and Example 2 is similar, and the amount of red blood cell adsorption of Example 3 is slightly lower than that of Examples 1 and 2, which indicates that the three groups of Examples all have certain procoagulant ability, and the procoagulant ability of Examples 1 and 2 is slightly higher than that of Example 3. The red blood cell concentrations of the supernatants of the control group and Examples 1 to 3 were 3.055×10 8 RCB / mL, 3.25×10 7 RCB / mL, 3.5×10 7 RCB / mL and 8.7×10 7 RCB / mL, and the red blood cell adhesion rate of the microspheres of the present invention is higher than 70%, indicating that the microspheres have obvious procoagulant function.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A pectin microsphere having both rapid hemostasis and wound healing properties, characterized in that: The microspheres are prepared from decellularized skin matrix, pectin and divalent cations through an emulsification cross-linking method.

2. The pectin microspheres having both rapid hemostasis and wound healing properties according to claim 1, characterized in that: The particle size of the microspheres is 10 to 100 μm.

3. The pectin microspheres having both rapid hemostasis and wound healing properties according to claim 1, characterized in that: The divalent cations include Ca 2+ Mg 2+ 、Zn 2+ , Cu 2+ or Mn 2+ .

4. A method for preparing pectin microspheres having both rapid hemostasis and wound healing properties as claimed in claim 1, characterized in that: The following steps are involved: 1) dissolving pectin in water to prepare a pectin solution with a mass concentration of 1 to 4%, then mixing the decellularized skin matrix solution and the pectin solution to obtain a matrix-pectin mixed solution for later use; 2) placing the oil phase in a water bath at 40-45° C., adding an emulsifier, stirring evenly, then dropping the matrix-pectin mixed solution obtained in step 1), maintaining the same temperature and speed, continuing stirring, then adding a cross-linking agent containing divalent cations, maintaining the same temperature and speed, continuing stirring, and obtaining a reaction product after the reaction is completed; 3) The reaction product obtained in step 2) is washed with petroleum ether and anhydrous ethanol for multiple times, and freeze-dried to obtain the pectin microspheres.

5. The method for preparing pectin microspheres having both rapid hemostasis and wound healing properties according to claim 4, characterized in that: The decellularized skin matrix solution is prepared by the following steps: taking animal dermal tissue, removing excess impurities and cutting into small pieces, removing subcutaneous fat and cleaning, and then soaking in a 0.25% trypsin solution for 12 hours, in 70% isopropanol containing 0.1% SDS for 12 hours, in 70% isopropanol containing 1% Triton X-100 for 12 hours, and in 100% isopropanol for 12 hours at 37°C, and then shaking and washing with a large amount of ionized water, freeze-drying, and then digesting the freeze-dried tissue with pepsin under acidic conditions. After the reaction is completed, centrifugation is performed to remove cell debris and other impurities to obtain a decellularized dermal matrix solution.

6. The method for preparing pectin microspheres having both rapid hemostasis and wound healing properties according to claim 4, characterized in that: The mass concentration ratio of the decellularized skin matrix to pectin in the matrix-pectin mixed solution is 1:10-40; and the pH value of the decellularized skin matrix solution is 7.0-7.

5.

7. The method for preparing pectin microspheres having both rapid hemostasis and wound healing properties according to claim 4, characterized in that: The oil phase is liquid paraffin or vegetable oil; the emulsifier is one or more of Span80 and Tween20, and the added amount of the emulsifier is 1% to 10% of the volume of the oil phase.

8. The method for preparing pectin microspheres having both rapid hemostasis and wound healing properties according to claim 4, characterized in that: The cross-linking agent containing divalent cations is calcium chloride, magnesium chloride or zinc chloride; the mass concentration of divalent cations in the cross-linking agent is 2-10%.

9. The method for preparing pectin microspheres having both rapid hemostasis and wound healing properties according to claim 4, characterized in that: The stirring speed in step 2) is 500-1000 rpm, and the stirring time is 30-60 min.

10. Use of the pectin microspheres according to any one of claims 1 to 3 or the pectin microspheres prepared by the method according to any one of claims 4 to 9 in the preparation of drugs related to hemostasis and skin repair.

Citation Information

Patent Citations

  • Skin wound healing preparation

    CN114073759A

  • Preparation method and application of blood cell active hydrogel for wound repair

    CN117482280A