Fe3O4-TiO2 magnetic nanosheet as well as preparation method and application thereof
Fe3O4-TiO2 magnetic nanosheets were prepared by sol-gel method and solvothermal method, which solved the problem of carrier recombination and agglomeration, achieved efficient catalytic degradation of dye wastewater, had good recyclability and stability, and significantly improved the catalytic efficiency active.
Patent Information
- Application Number
- CN202410793602.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-19
AI Technical Summary
Existing Fe3O4-TiO2 nanocomposites have problems with easy recombination and agglomeration of carriers in the catalyst, which affects the catalytic activity, and it is difficult to control the morphology and dispersion with traditional preparation methods, limiting their application potential.
A combination of sol-gel method and solvothermal method was used to prepare Fe3O4-TiO2 magnetic nanosheets with different TiO2 loading rates. TiO2 and Fe3O4 were closely connected through chemical bonds to form a unique two-dimensional nanostructure, which promoted the transfer of photogenerated electrons and inhibited electron- Holes recombine to improve catalytic activity.
Achieved high-efficiency catalytic degradation of dye wastewater, with good recyclability and stability, significantly improved the conversion efficiency of Fe3+/Fe2+ and the photocatalytic activity of TiO2. The catalyst still maintains a degradation rate and recovery of more than 90% after 5 cycles. Rate.
Smart Images

Figure BDA0004900807280000071 
Figure HDA0004900807290000011 
Figure HDA0004900807290000012
Abstract
Description
Technical Field
[0001] The invention relates to a Fe3O4-TiO2 magnetic nanosheet and a preparation method and application thereof, belonging to the technical field of inorganic nanomaterial preparation / nanocomposite materials. Background Art
[0002] Nanocomposites are a trend in recent years. Compared with single materials, nanocomposites have the functions of multiple materials and can achieve the effect of taking advantage of each other's strengths and making up for each other's weaknesses. Nanocomposites with magnetic nanoparticles as carriers have attracted widespread attention due to their excellent magnetic properties and simple preparation. In addition, if these magnetic nanocomposites are applied to catalytic systems, they can be separated from the reaction system by external magnets, which not only avoids the problems of expensive equipment costs and long separation time caused by separation processes such as centrifugation, but also reduces the loss of catalysts and facilitates the recycling of catalysts.
[0003] At present, most researchers combine the photocatalyst TiO2 with the Fenton-like catalyst Fe3O4. The photogenerated - Can be transferred to Fe 3+ On the Fe 3+ / Fe 2+ The conversion rate of photogenerated e in TiO2 is inhibited - -h + The combination of Fe3O4 and TiO2 produces more active species, which catalyzes the oxidation and degradation of organic pollutants. However, ordinary Fe3O4 nanoparticles have defects such as easy recombination of carriers and easy aggregation in solution, which seriously affect the catalytic activity. In recent years, two-dimensional transition metal oxides have shown good application prospects in electrocatalysis, electronic devices and energy storage due to their inherent quantum confinement characteristics of electrons. Fe3O4 nanosheets have a unique two-dimensional nanostructure and not only have a larger specific surface area, which is conducive to the deposition and loading of TiO2 nanoparticles and exposes more active sites, but also the layered structure of the supporting matrix can effectively inhibit the agglomeration of nanoparticles. In addition, it has a faster electron transfer rate, which provides a huge opportunity for the development of new and efficient catalysts.
[0004] At present, the methods for preparing Fe3O4-TiO2 nanocomposite materials mainly include precipitation method, sol-gel method and solvent thermal / hydrothermal method. Among them, the precipitation method is to add a suitable precipitant to a soluble salt solution, hydrolyze at a certain temperature, precipitate an insoluble precipitate, wash, dry and calcine to obtain the desired nanoparticles. Although this method has a wide range of raw materials, does not involve high temperature and high pressure, and has low cost, it lays a foundation for large-scale production, but the samples prepared by this method are easy to agglomerate, poor in dispersibility, and difficult to control in morphology, so there is still room for further optimization. Sol-gel method refers to a method of using metal alkoxide as a precursor, through hydrolysis and condensation chemical reactions, forming a stable sol system, through aging reaction, forming a gel, and the gel is dried, sintered and solidified to prepare a product. Compared with other methods, the sol-gel method can obtain molecular level uniformity in a very short time when forming a gel, and the reaction conditions are mild, the preparation is simple, and it has broad application prospects. Solvothermal / hydrothermal method refers to a synthesis method in which the original mixture reacts at a certain temperature and autogenous pressure of the solution in a closed high-pressure reactor with non-aqueous / aqueous medium as solvent. The samples prepared by this method have good dispersibility and crystallinity, and can improve the catalytic degradation efficiency of organic pollutants in wastewater. Therefore, the use of appropriate methods to prepare Fe3O4-TiO2 nanosheets with excellent magnetic and photocatalytic properties has become the current research focus. Summary of the invention
[0005] The purpose of the present invention is to provide a Fe3O4-TiO2 magnetic nanosheet. The present invention adopts a sol-gel method and a solvothermal method to prepare Fe3O4-TiO2 nanosheets with different TiO2 loading rates, which are used for catalytic degradation of dye wastewater. The unique two-dimensional nanostructure of the Fe3O4 nanosheet enables it to have a better interaction with TiO2 nanoparticles, promoting the photogenerated electrons in TiO2 to effectively transfer Fe 3+ Reduction to Fe 2+ , which increases Fe 3+ / Fe 2+ conversion efficiency and photocatalytic activity of TiO2.
[0006] The effective combination of photocatalysis and Fenton-like reaction under the catalysis of the Fe3O4-TiO2 magnetic nanosheets of the present invention not only makes the Fe3O4-TiO2 nanosheets have excellent catalytic degradation efficiency but also gives them good recyclability and stability. The Fe3O4-TiO2 nanosheets of the present invention not only achieve efficient degradation of RhB dye wastewater, but also can be reused many times, significantly reducing costs, laying a foundation for its practical application.
[0007] The preparation method of Fe3O4-TiO2 magnetic nanosheets provided by the present invention comprises the following steps:
[0008] S1, adding ammonia water to the dispersion of Fe3O4 magnetic nanosheets;
[0009] S2, adding a solution of butyl titanate (TBOT) dropwise to the solution obtained in step S1 to react;
[0010] S3. After dispersing the product obtained in step S2, adding ammonia water, and then placing it in a reactor for heat treatment, Fe3O4-TiO2 magnetic nanosheets are obtained.
[0011] In the above preparation method, in step S1, a dispersion of the Fe3O4 magnetic nanosheets is prepared using a mixed solution of ethanol and acetonitrile;
[0012] In the dispersion, the mass-volume concentration of the Fe3O4 magnetic nanosheets is 0 to 2 mg / mL, preferably 1 mg / mL;
[0013] The mass concentration of the ammonia water is 25-28%;
[0014] The volume ratio of the aqueous ammonia to the dispersion is 0.25 to 1:100, preferably 0.5:100.
[0015] In the above-mentioned preparation method, in step S2, a mixture of ethanol and acetonitrile is used to prepare the solution of butyl titanate;
[0016] Using a syringe to drop the solution of butyl titanate into the solution;
[0017] The dosage of the butyl titanate is 0.25-1.25 mL / 100 mg Fe3O4 magnetic nanosheets, preferably 0.75 mL / 100 mg Fe3O4 magnetic nanosheets.
[0018] The reaction temperature is room temperature, and the reaction time is 1 to 4 hours, preferably 2 hours.
[0019] In the above preparation method, in step S3, the product obtained in step S2 is dispersed in a mixed solution of ethanol and water, the aqueous ammonia is added under ultrasonic conditions, and the ultrasonic treatment is continued for 10 to 25 minutes before being transferred to the reactor.
[0020] In the above preparation method, in step S3, the heat treatment temperature is 120-180° C. and the time is 20-26 hours.
[0021] In the above preparation method, in step S3, the Fe3O4-TiO2 magnetic nanosheets are separated from the heat-treated system by magnetic separation, and then washed several times with deionized water and anhydrous ethanol, and then placed in a freeze dryer for freeze drying.
[0022] The present invention constructs a photocatalytic synergistic Fenton-like reaction system based on Fe3O4-TiO2 magnetic nanosheets, which can be applied to catalytic degradation of dye wastewater, such as RhB dye wastewater.
[0023] In the Fe3O4-TiO2 magnetic nanosheet provided by the present invention, TiO2 and Fe3O4 are tightly connected via chemical bonds, and the interface structure can induce the nanosheet to produce more active sites, thereby improving the catalytic performance thereof.
[0024] In the present invention, after Fe3O4 is introduced into the catalyst TiO2, the existence of Ti-O-Fe bonds changes the transfer path of photogenerated carriers and inhibits the photogenerated e - -h + The catalytic activity of the catalyst is improved.
[0025] Under the action of an external magnetic field, the Fe3O4-TiO2 magnetic nanosheets of the present invention can be quickly separated from the dispersed solution, indicating that they have sufficient magnetism. The Fe3O4-TiO2 magnetic nanosheets of the present invention have good reusability.
[0026] The Fe3O4-TiO2 magnetic nanosheets of the present invention overcome the limitations of traditional Fe3O4 nanoparticles and have the advantages of simple preparation, reusability, high catalytic degradation efficiency, etc. The unique two-dimensional nanostructure of the Fe3O4-TiO2 magnetic nanosheets of the present invention enables them to have better interaction with TiO2 nanoparticles, promoting the photogenerated electrons in TiO2 to effectively convert Fe 3+ Reduction to Fe 2 + , inhibiting the recombination of photogenerated electron-hole pairs and improving the catalytic activity of the catalyst. The synergistic effect of the photocatalysis and Fenton-like reaction of the Fe3O4-TiO2 magnetic nanosheets of the present invention can significantly improve the degradation efficiency of the RhB dye. Based on the good magnetic properties and high catalytic activity of the Fe3O4-TiO2 magnetic nanosheets of the present invention, it has excellent recyclability and stability. After 5 cycles, the photocatalytic degradation rate and recovery rate of the system are still more than 90%. The present invention realizes the efficient, rapid and low-cost degradation of RhB and other dye wastewaters, and provides a new research idea for the design and application of wastewater catalytic degradation materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the synthesis of Fe3O4-TiO2 nanosheets according to the present invention.
[0028] Figure 2 Figure 2 is the N2 adsorption-desorption curve (Figure a) and pore size distribution curve (Figure b) of Fe3O4-TiO2 of the present invention.
[0029] Figure 3 XRD spectra of different samples.
[0030] Figure 4 This is the XPS spectrum of FT-0.75 (figures ad are survey, Fe 2p, Ti 2p and O1s respectively).
[0031] Figure 5 The SEM image of Fe3O4 (Figure a), the SEM image of FT-0.75 (Figure b), the TEM image of FT-0.75 (Figure c) and the HRTEM image of FT-0.75 (Figure d).
[0032] Figure 6 UV-vis spectrum (Figure a), Tauc plot (Figure b) and PL emission spectrum (Figure c) of the catalyst sample.
[0033] Figure 7 The degradation rate of RhB dye by Fe3O4-TiO2 (Figure a), the changes in the UV-visible absorption spectrum of RhB dye solution at different time intervals (Figure b), the photographic records of RhB dye solution at different time intervals (Figure c), the degradation of RhB dye under different systems (Figure d) and the corresponding reaction rate constant k under different systems (Figure e).
[0034] Figure 8 The MH curves of Fe3O4 and FT-0.75 (Figure a, the upper left inset is the MH curve under low magnetic field, and the lower right inset is the magnetic separation photo), the cyclic experiment of RhB dye degradation by FT-0.75+H2O2+light system (Figure b), and the XRD spectrum of FT-0.75 before and after the cyclic experiment (Figure c). DETAILED DESCRIPTION
[0035] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0036] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0037] Example 1. Synthesis and Characterization of TiO2 Nanoparticles and Fe3O4-TiO2 Nanosheets
[0038] 1. Synthesis Schematic Diagram Figure 1 shown.
[0039] Disperse Fe3O4 magnetic nanosheets (100 mg) in 100 mL of anhydrous ethanol / acetonitrile mixed solution (3 / 1, v / v), sonicate to fully dissolve, then add NH3·H2O solution (0.50 mL), continue sonication, and transfer to a three-necked flask after fully dissolving, with the stirring speed set to 500 rpm. Add TBOT solution dropwise to 20 mL of anhydrous ethanol / acetonitrile mixed solution (3 / 1, v / v), stir magnetically for 30 min, then transfer to a 20 mL syringe, install the syringe on a syringe pump, set the syringe pump's drop time to 20 min, and push it dropwise into the three-necked flask. After the dropwise addition is completed, continue the reaction for 2 h. After the reaction is completed, separate and wash the product. The obtained product was then dispersed in anhydrous ethanol (40 mL) and deionized water (20 mL), and NH3·H2O solution (2.5 mL) was added under ultrasonic conditions. After ultrasonic treatment for 15 min, the mixture was transferred to a 100 mL reactor and heat treated at 160°C for 24 h. After the high-pressure reactor was naturally cooled to room temperature, the product was separated by a magnet, and the obtained product was washed several times with deionized water and anhydrous ethanol, and the product was placed in a freeze dryer for freeze drying for 48 h.
[0040] The amount of TBOT solution added (TBOT dosage: 0.25, 0.5, 0.75, 1, 1.25 mL / 100 mg Fe3O4 magnetic nanosheets) was 0.25, 0.5, 0.75, 1 and 1.25 mL, respectively, and the corresponding nanosheets were labeled as FT-0.25, FT-0.5, FT-0.75, FT-1 and FT-1.25. If Fe3O4 nanoparticles are used, it is defined as SFT-0.75. The synthesized sample without Fe3O4 magnetic nanosheets is pure TiO2 nanoparticles.
[0041] 2. Structure and surface composition of Fe3O4 magnetic nanosheets
[0042] Figure 2 N2 adsorption-desorption isotherms and BJH pore size distribution diagrams of Fe3O4-TiO2 nanosheets prepared with different TBOT dosages.
[0043] from Figure 2 As can be seen in Figure a, according to the IUPAC classification, the N2 adsorption-desorption isotherms of all catalyst samples are type IV, with an H3 hysteresis loop, which is a mesoporous structure. Figure 2Figure b shows that there are a large number of mesopores with pore sizes ranging from 2 to 50 nm in the catalyst sample. More importantly, the specific surface area and pore volume of the catalyst sample increase first and then decrease with the increase of the TiO2 ratio. This may be due to the stacking of an appropriate amount of TiO2 nanoparticles on the surface of the Fe3O4 magnetic nanosheets to form a large number of new mesopores, which increases the pore volume. However, when the TiO2 nanoparticles are excessive, some of the original pores will be masked, which will lead to a decrease in the pore volume. When the TBOT dosage is 0.75 mL, the specific surface area (121.67 m 2 ·g -1 ) and pore volume (0.554 cm 3 ·g -1 ) is the largest. The large specific surface area and rich pore structure are conducive to increasing its contact area with pollutants, thereby enhancing its adsorption and catalytic degradation performance of target pollutants. Therefore, FT-0.75 nanosheets are considered to be a good adsorption and photocatalytic material.
[0044] Figure 3 XRD spectra of TiO2 nanoparticles, Fe3O4 nanosheets and FT-0.75 nanosheets.
[0045] The XRD spectrum of TiO2 nanoparticles shows that the characteristic peaks at 2θ of 25.281°, 37.800°, 48.049°, 53.890°, 55.060°, 62.688°, 68.760°, 70.309° and 75.029° correspond to the (101), (004), (200), (105), (211), (204), (116), (220) and (215) crystal planes of anatase phase titanium dioxide (JCPDF No.21-1272). Compared with rutile, anatase TiO2 is more conducive to the adsorption and photocatalytic oxidation of organic pollutants because it has a slower electron-hole pair recombination rate and a higher reduction potential. For Fe3O4 magnetic nanosheets, several characteristic peaks at 30.091°, 35.443°, 43.074°, 53.438°, 56.964° and 62.553° are consistent with the (220), (311), (400), (422), (511) and (440) crystal planes of cubic magnetite Fe3O4 (JCPDF 85-1436). These peaks are sharp and intense, and there are no other redundant peaks, which proves that the prepared samples are of high purity and good crystallinity. From the XRD spectrum of FT-0.75 nanosheets, it can be seen that in addition to the diffraction peaks caused by Fe3O4, there are also diffraction peaks of anatase TiO2, and after loading TiO2 nanoparticles, the diffraction peaks of Fe3O4 remain basically unchanged, indicating that the introduction of TiO2 nanoparticles has no effect on the crystal structure of Fe3O4 magnetic nanosheets.
[0046] In order to further verify the elemental composition and chemical state of the surface of FT-0.75 nanosheets, XPS tests were performed on FT-0.75 nanosheets. The results are as follows Figure 4 shown.
[0047] Figure 4 Figure a in the middle is the full spectrum of FT-0.75. It can be seen from the figure that Fe, Ti and O elements exist in FT-0.75. Figure 4 b shows the Fe 2p spectrum. 3 / 2 and Fe 2p 1 / 2 The binding energies of Fe 2+ (from FeO) and Fe 3+ (from Fe2O3) peak composition, indicating the presence of Fe3O4 in the nanosheets. Figure 4 Figure c shows the Ti 2p spectrum, where Ti2p 3 / 2 and Ti 2p 1 / 2 There are two obvious peaks at 458.4eV and 464.2eV, respectively, which are consistent with the Ti 4+ phase, indicating the formation of anatase TiO2. Figure 4 Figure d in the middle is the O1s spectrum, and an obvious peak appears at 530.1eV, which corresponds to the bond energy of the Ti-O-Fe bond. The existence of the Ti-O-Fe bond indicates that the combination of Fe3O4 and TiO2 is not a simple physical mixture, but is tightly bound through chemical bonds, which makes the FT-0.75 nanosheets have strong stability.
[0048] The morphology of the catalyst samples was characterized by scanning electron microscopy and transmission electron microscopy. Figure 5 shown.
[0049] like Figure 5 As shown in Figure a, the Fe3O4 catalyst sample is composed of polygonal nanosheets, and the majority of nanosheets are hexagonal. Figure 5 As can be seen in Figure b, TiO2 nanoparticles with a particle size of about 10 to 20 nm are uniformly deposited and loaded on the Fe3O4 magnetic nanosheets. Due to the deposition and coating of a large number of TiO2 nanoparticles on the Fe3O4 magnetic nanosheets, the FT-0.75 nanosheets present an irregular polygonal sheet structure. Figure 5 Figure c is a TEM image of FT-0.75 nanosheets, which further shows that FT-0.75 nanosheets are composed of Fe3O4 nanosheets and TiO2 nanoparticles. Figure 5As shown in Figure d, the lattice spacing further confirms that the FT-0.75 nanosheets have two different crystal planes. Combined with the previous XRD analysis, the lattice spacing of 0.296nm corresponds to the (220) plane of Fe3O4, and 0.3523nm corresponds to the (101) plane of TiO2. In addition, it is worth noting that a connection is observed at the intersection of two different lattice spacings between Fe3O4 and TiO2, indicating that TiO2 nanoparticles are successfully deposited on the surface of Fe3O4 magnetic nanosheets. According to the previous XPS spectrum analysis, Ti-O-Fe bonds are formed at the intersection of Fe3O4 and TiO2, further indicating that TiO2 and Fe3O4 are tightly connected through chemical bonds, and the interface structure can induce FT-0.75 nanosheets to produce more active sites, thereby improving their catalytic performance.
[0050] 3. Optical and photoelectrochemical properties of Fe3O4 magnetic nanosheets
[0051] To study the light absorption capacity of the catalyst, the catalyst samples were subjected to UV-visible diffuse reflectance tests. Figure 6 shown.
[0052] like Figure 6 As shown in Figure a, TiO2 has a strong light absorption edge in the ultraviolet region, and the absorption edge is located at 382nm. The bandgap width of Fe3O4 is 0.1eV, which is a narrow-band semiconductor, so its light absorption capacity in the visible light region is more significant. After TiO2 nanoparticles are loaded onto the surface of Fe3O4 magnetic nanosheets, the absorption band edge of FT-0.75 nanosheets relative to TiO2 shows a significant red shift, proving that the introduction of narrow-bandgap semiconductors can effectively improve the visible light absorption capacity of photocatalysts. Figure 6 Figure b in the middle shows the energy gap of the catalyst sample, which is Figure 6 As shown in Figure b, the estimated band gaps of TiO2 and FT-0.75 are 3.25 eV and 1.65 eV, respectively, which can be attributed to the Fe 3+ (0.1064nm) has an ionic radius close to that of Ti 4+ (0.1068nm), during the recombination process, some Fe 3+ Can replace Ti 4+ The lattice position of TiO2 is changed to produce lattice defects, forming a new impurity band, which causes the valence band position of TiO2 to move up, while the conduction band position remains unchanged, the bandgap width becomes smaller, and the light response range is expanded.
[0053] In order to study the charge separation efficiency of the catalyst samples, the PL spectra of the catalyst samples were measured at an excitation wavelength of 385 nm, as shown in Figure 6As shown in Figure c, TiO2 nanoparticles exhibit a higher PL intensity signal, indicating that electron-hole pairs are easy to recombine. The PL intensity signals of SFT-0.75 and FT-0.75 are relatively low, indicating that the introduction of Fe3O4 into the catalyst TiO2 enhances the photogenerated electrons. - -h + The separation ability of the pairs makes it less likely to recombine. In contrast, the PL intensity signal of FT-0.75 is the lowest. This can be attributed to the fact that the Fe3O4 magnetic nanosheets are controlled by a specific crystal plane, and the unique surface structure makes it have a large contact area with the TiO2 nanoparticles, thus promoting the photogenerated - Transfer from TiO2 nanoparticles to Fe3O4 magnetic nanosheets, photogenerated - -h + The separation efficiency is higher and the photocatalytic activity is higher. In addition, after the introduction of Fe3O4 into the catalyst TiO2, the presence of Ti-O-Fe bonds changes the transfer path of photogenerated carriers and inhibits the photogenerated e - -h + The catalytic activity of the catalyst is improved.
[0054] Example 2: Photocatalytic degradation performance of FT-0.75 in synergistic Fenton-like reaction
[0055] 1. Photocatalytic synergistic Fenton-like reaction experiment
[0056] The UV analyzer was selected as the light source and the RhB dye solution was selected as the target pollutant. The catalytic degradation effect of Fe3O4-TiO2 nanosheets was evaluated by measuring the decolorization of the RhB dye solution under light irradiation.
[0057] Specific catalytic degradation experimental steps: Weigh a certain amount of Fe3O4-TiO2 nanosheets as catalyst and place them in 100mL, 30mg·L -1 The RhB dye solution was stirred and protected from light for 30 minutes to allow the Fe3O4-TiO2 nanosheets to reach adsorption-desorption equilibrium with the dye. The supernatant was separated by magnetism, and the absorbance of the RhB dye solution was detected at a peak absorption wavelength of 553nm using a UV-visible spectrophotometer. Then a certain amount of H2O2 was added, and the light source was turned on to start the photocatalytic degradation reaction. Every 20 minutes, the supernatant was separated by magnetism, the absorbance was detected, and converted into concentration according to the Lambert-Beer law, and its degradation rate was calculated.
[0058] The calculation method of the degradation rate of RhB dye solution is shown in formula (1):
[0059]
[0060] Where C0 is the initial concentration of the RhB dye solution after the dark reaction is completed and before illumination, in mg·L -1 ; C is the concentration of RhB dye solution at time t of illumination, in mg·L -1 .
[0061] 2. Photocatalytic degradation performance of FT-0.75 in synergistic Fenton-like reaction
[0062] Firstly, the effect of Fe3O4-TiO2 nanosheets prepared at different TBOT dosages on the catalytic degradation of RhB dye solution was investigated. Figure 7 shown.
[0063] like Figure 7 As shown in Figure a, with the increase of TBOT dosage, the degradation behavior of Fe3O4-TiO2 nanosheets of the present invention on RhB dye shows a trend of first increasing and then decreasing. The degradation efficiency of FT-0.75 nanosheets is the highest, reaching 98.12%. This can be attributed to the higher specific surface area of FT-0.75 and the effective separation of electron-hole pairs. At the same time, Figure 7 Middle B picture and Figure 7 Figure c shows the changes in the absorption spectrum of the RhB dye solution exposed to light at different time intervals under the action of FT-0.75 nanosheets and the corresponding photographic records. The main absorption peak of RhB at 553nm decreases with the increase of irradiation time, and the color of the RhB dye solution gradually becomes lighter until it is close to transparent, indicating that the RhB dye is removed. FT-0.75 nanosheets show higher degradation efficiency.
[0064] In order to further illustrate the effectiveness of the FT-0.75 photocatalytic synergistic Fenton-like system, the present invention conducted a series of experiments to study the degradation of RhB dye by different reaction systems. Figure 7 As shown in Figure d, when light is used alone, the concentration of RhB dye remains almost unchanged and the self-photolysis effect can be ignored. For the H2O2+light system, since light irradiation can promote the decomposition of H2O2 to produce active substances ·OH, the degradation rate can reach 43.12%. After adding photocatalysts TiO2 and FT-0.75 under light conditions, a photocatalytic oxidation reaction occurs, and the degradation rate is further improved. Moreover, the degradation rate of the photocatalytic system with FT-0.75 as the catalyst (65.91%) is higher than the degradation rate of the photocatalytic system with TiO2 as the catalyst (51.01%). This is mainly because the Fe in the Fe3O4 magnetic nanosheets 3+ It captures the photogenerated - Fe 2+ , inhibiting the photogenerated - -h +The photocatalytic performance of the composite was improved. For the heterogeneous photo-Fenton system (Fe3O4+H2O2+light), the degradation rate of RhB dye could reach 76.36%. For the photocatalytic synergistic Fenton system (FT-0.75+H2O2+light), the degradation rate of RhB dye was further improved to 98.12%. This may be due to the unique two-dimensional nanostructure of Fe3O4 magnetic nanosheets, which is conducive to its good interaction with TiO2 nanoparticles. The photogenerated electrons generated by TiO2 under light interact with Fe 3+ The reaction generates Fe 2+ , which promotes Fe 3+ / Fe 2 + The cycle of photocatalytic reaction increases the rate of Fenton-like reaction. At the same time, the recombination of photogenerated electron-hole pairs is also suppressed during the photocatalytic reaction, further increasing the reaction rate.
[0065] In order to make a more comprehensive comparison, the catalytic degradation data of RhB dye were further analyzed using the fitted first-order kinetic equation:
[0066] -ln(C / C0)=k×t (2)
[0067] Among them, C (mg·L -1 )、C0(mg·L -1 )、t(min)、k(min -1 ) are respectively the concentration of RhB dye after irradiation, the initial concentration of RhB dye, the irradiation time, and the reaction rate constant. Figure 7 As shown in Figure e, the k value of FT-0.75+H2O2+light (0.03301min -1 ) are FT-0.75+light(0.008680min -1 ) and Fe3O4+H2O2+light(0.01209min -1 ), which further illustrates that in the FT-0.75+H2O2+light system, photocatalysis and Fenton-like reaction have a synergistic effect, which further improves the reaction rate.
[0068] 3. Reusability and stability of FT-0.75 nanosheets
[0069] The reusability and stability of catalysts are important factors affecting their practical applications. Figure 8 Figure a shows the hysteresis loop of the catalyst sample measured by VSM. The residual magnetization of FT-0.75 nanosheets (3.27 emu g -1) and coercivity (58.4Oe) are negligible, indicating that it has typical superparamagnetism. The saturation magnetization of Fe3O4 nanosheets is 68.3emu·g -1 After the deposition of TiO2 nanoparticles, the magnetic properties of FT-0.75 nanosheets decreased, and the saturation magnetization was 34.5emu·g -1 Nevertheless, under the action of an external magnetic field, FT-0.75 nanosheets can be quickly separated from the dispersed solution, indicating that they have sufficient magnetic properties.
[0070] The reusability of FT-0.75 nanosheets in a photocatalytic synergistic Fenton-like system was evaluated by a RhB dye degradation cycle experiment. After each cycle, the catalyst was separated from the solution by a magnet, washed, dried, and used in the next cycle while keeping other reaction conditions unchanged. Figure 8 As shown in Figure b, as the number of cycles increases, the recovery rate of FT-0.75 nanosheets decreases, which may be due to the loss of catalyst during the cleaning process. In addition, the catalytic degradation rate of RhB dye by FT-0.75 nanosheets decreases. This may be because after the cycle, the pollutants are adsorbed on the catalyst surface, the active sites are reduced, and thus the degradation efficiency of RhB dye is affected. However, after 5 cycles, the recovery rate of FT-0.75 nanosheets and the degradation rate of RhB dye can still exceed 90%, indicating that FT-0.75 nanosheets have good reusability.
[0071] In addition, the excellent stability of FT-0.75 nanosheets can also be observed from the fresh and used XRD patterns (e.g. Figure 8 As shown in Figure c), there is no significant difference in the crystal structure of the FT-0.75 nanosheet before and after 5 cycles. Therefore, the FT-0.75 nanosheet provided by the present invention can be used as an efficient and recyclable catalyst for wastewater treatment of organic pollutants.
Claims
1. A kind of Fe 3 O 4 -TiO 2 The method for preparing magnetic nanosheets comprises the following steps: S1. Add ammonia to Fe 3 O 4 In the dispersion of magnetic nanosheets; S2, adding the solution of butyl titanate dropwise to the solution obtained in step S1 to react; S3, after dispersing the product obtained in step S2, adding ammonia water, and then placing it in a reactor for heat treatment, to obtain Fe 3 O 4 -TiO 2 Magnetic nanosheets.
2. The preparation method according to claim 1, Features: In step S1, a mixture of ethanol and acetonitrile is used to prepare the Fe 3 O 4 a dispersion of magnetic nanosheets; In the dispersion, the Fe 3 O 4 The mass-volume concentration of magnetic nanosheets is 0 to 2 mg / mL; The mass concentration of the ammonia water is 25-28%; The volume ratio of the ammonia water to the dispersion liquid is 0.25 to 1:
100.
3. The preparation method according to claim 1 or 2, Features: In step S2, a mixture of ethanol and acetonitrile is used to prepare the butyl titanate solution; Using a syringe to drop the solution of butyl titanate into the solution; The dosage of the titanate is: 0.25-1.25 mL / 100 mg Fe 3 O 4 Magnetic nanosheets; The reaction temperature is room temperature and the reaction time is 1 to 4 hours.
4. The preparation method according to any one of claims 1 to 3, Features: In step S3, the product obtained in step S2 is dispersed in a mixed solution of ethanol and water, and the aqueous ammonia is added under ultrasonic conditions, and the ultrasonic treatment is continued for 10 to 25 minutes before being transferred to the reactor.
5. The preparation method according to any one of claims 1 to 4, Features: In step S3, the heat treatment is carried out at a temperature of 120 to 180° C. and for a time of 20 to 26 hours.
6. The preparation method according to any one of claims 1 to 5, Features: In step S3, the Fe 3 O 4 -TiO 2 Magnetic nanosheets.
7. Fe prepared by the method according to any one of claims 1 to 6 3 O 4 -TiO 2 Magnetic nanosheets.
8. Fe according to claim 7 3 O 4 -TiO 2 Application of magnetic nanosheets as catalysts in photocatalytic synergistic Fenton-like reaction for dye wastewater treatment.
Citation Information
Patent Citations
Method for manufacturing magnetic loading type nanometer catalyst TiO2 / Fe2O4
CN101816937A
Preparation and application of novel easy-to-recycle high-efficient visible light catalyst
CN102671662A
Preparation method and application of magnetic graphene titanium dioxide nano composite wastewater treatment agent
CN107445387A
Preparation of TiO2-Fe3O4 magnetic material and application of TiO2-Fe3O4 magnetic material in degradation of potato starch wastewater