By using CdIn2S4/ZnO composite material as an acoustic catalyst in wastewater, the efficiency and safety issues of antibiotic treatment in wastewater were solved, and efficient degradation of tetracycline hydrochloride was achieved, demonstrating the superiority of the composite material in water pollution treatment.

CN118719093AInactive Publication Date: 2024-10-01LIAONING UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410783657.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technology is difficult to efficiently and safely treat antibiotics, such as tetracyclines, in wastewater, leading to the emergence of drug-resistant pathogenic bacteria, and traditional treatment methods have safety and environmental issues.

Method used

CdIn2S4/ZnO composite material was used as an acoustic catalyst, prepared through hydrothermal reaction, and the composite material was used to degrade organic pollutants in wastewater, including tetracycline hydrochloride, under ultrasonic conditions.

Benefits of technology

It achieves efficient degradation of tetracycline hydrochloride, has good safety and environmental protection, and improves the effect of water pollution treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719093A_ABST
    Figure CN118719093A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid ultrasonic catalysis, and particularly relates to a CdIn2S4 / ZnO composite material as well as a preparation method and application thereof. According to the CdIn2S4 / ZnO composite material, the mass ratio of CdIn2S4 in ZnO is 20%-50%. The prepared CdIn2S4 / ZnO composite material is combined with ultrasonic to degrade tetracycline in water, the ultrasonic power is 500 W, the ultrasonic time is 2 h, and the degradation rate of tetracycline hydrochloride in water can reach 91.03 + / -1.41%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid ultrasonic catalysis, and specifically relates to a CdIn2S4 / ZnO composite material and a preparation method and application thereof. Background Art

[0002] Antibiotics remaining in the environment can induce pathogenic microorganisms to produce drug-resistant genes, leading to the emergence of drug-resistant pathogens. Drug-resistant pathogens pose a huge threat to human health, especially super pathogens with multidrug resistance. Among antibiotics, tetracycline ranks among the most used. Therefore, it is particularly important to efficiently and safely treat tetracycline in wastewater. Summary of the invention

[0003] The purpose of the present invention is to provide a CdIn2S4 / ZnO composite material with good degradation effect, green and safe, which has a good application prospect as an efficient and environmentally friendly acoustic catalyst for effectively solving water pollution.

[0004] The technical solution adopted by the present invention is: a CdIn2S4 / ZnO composite material, wherein the mass ratio of CdIn2S4 in ZnO is 20%-50%.

[0005] The above-mentioned CdIn2S4 / ZnO composite material is prepared by dissolving ZnO, Cd(NO3)2·4H2O, TAA and InCl3·4H2O in deionized water and stirring to carry out a hydrothermal reaction. The precipitate obtained by the reaction is washed three times with deionized water and anhydrous ethanol respectively, and then the product is dried to obtain the CdIn2S4 / ZnO composite material.

[0006] In the above-mentioned method for preparing a CdIn2S4 / ZnO composite material, the molar ratio of Cd(NO3)2·4H2O, TAA and InCl3·4H2O is 1:6:2.

[0007] In the above-mentioned method for preparing a CdIn2S4 / ZnO composite material, the hydrothermal reaction conditions are: the temperature is 180°C and the reaction time is 16 hours.

[0008] In the above-mentioned method for preparing a CdIn2S4 / ZnO composite material, the drying temperature is 80°C and the drying time is 16 hours.

[0009] The above-mentioned CdIn2S4 / ZnO composite material is used for ultrasonic catalytic degradation of organic pollutants in wastewater.

[0010] The application of the above-mentioned CdIn2S4 / ZnO composite material in ultrasonic catalytic degradation of organic pollutants in wastewater is as follows: adding the CdIn2S4 / ZnO composite material to the wastewater containing organic pollutants, and ultrasonicating for 2 hours at an ultrasonic power of 500W.

[0011] The above-mentioned CdIn2S4 / ZnO composite material is used in the ultrasonic catalytic degradation of organic pollutants in wastewater, and the initial concentration of the organic pollutants is 30 mg / L.

[0012] The above-mentioned CdIn2S4 / ZnO composite material is used in ultrasonic catalytic degradation of organic pollutants in wastewater, wherein the organic pollutant is tetracycline hydrochloride.

[0013] The above-mentioned CdIn2S4 / ZnO composite material is used for ultrasonic catalytic degradation of organic pollutants in wastewater, and the added amount of the CdIn2S4 / ZnO composite material is 0-3g / L.

[0014] The beneficial effect of the present invention is that both ZnO and CdIn2S4 have catalytic activity. After the two are compounded, the present invention adds different masses of CdIn2S4 / ZnO composite materials and combines them with ultrasonic degradation of tetracycline hydrochloride. The results show that the prepared CdIn2S4 / ZnO composite materials have the advantages of good degradation effect, no toxicity, high safety, etc., and have good application prospects in ultrasonic catalytic treatment of organic pollutants in wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 1 is the XRD spectrum of the CdIn2S4 / ZnO composite materials with different composite ratios obtained in Example 1.

[0016] Figure 2 These are scanning electron microscope (SEM) spectra of (A) ZnO, (B) CdIn2S4, and (C) CdIn2S4 / ZnOCZ-40 composite materials.

[0017] Figure 3 This is a comparison chart of the effects of stirring adsorption and synergistic ultrasonic catalytic degradation of tetracycline hydrochloride by CdIn2S4 / ZnO composites with different composite ratios.

[0018] Figure 4 This is a comparison chart of the effects of stirring adsorption and synergistic ultrasonic catalytic degradation of tetracycline hydrochloride by CdIn2S4 / ZnO composite material CZ-40 with different addition amounts and a composite ratio of 40%.

[0019] Specific example method

[0020] The present invention is described in detail below with reference to the embodiments.

[0021] Example 1

[0022] (I) Preparation of CdIn2S4 / ZnO composites with different composite ratios

[0023] 1) Preparation of CdIn2S4: Weigh 0.65 mol of Cd(NO3)2·4H2O, 4.46 mol of TAA and 1 mol of InCl3·4H2O, dissolve in a wide-mouth conical flask filled with 70 mL of deionized water and stir for 2 hours. The resulting mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and subjected to hydrothermal reaction at 180°C for 16 hours. The resulting precipitate was washed three times with deionized water and ethanol, respectively, and then dried at 80°C for 16 hours to obtain orange-yellow pure substance CdIn2S4.

[0024] 2) Preparation of CdIn2S4 / ZnO composite materials: 500 mg of ZnO and a certain mass of Cd(NO3)2·4H2O, TAA and InCl3·4H2O calculated according to different composite ratios were dissolved in a wide-mouth conical flask filled with 70 mL of deionized water and stirred for 2 hours. The resulting mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and subjected to hydrothermal reaction at 180°C for 16 hours. The precipitate obtained by the reaction was washed three times with deionized water and ethanol, respectively, and then dried at 80°C for 16 hours to obtain orange-yellow CdIn2S4 / ZnO composite materials with different composite ratios.

[0025] According to the different mass ratios of CdIn2S4 in ZnO (20%, 30%, 40%, 50% respectively, the corresponding mass of Cd(NO3)2·4H2O is 57.50mg, 86.24mg, 115.00mg, 143.75mg; the mass of TAA is 95.86mg, 143.79mg, 191.72mg, 239.65mg; the mass of InCl3·4H2O is 124.71mg, 187.07mg, 249.42mg, 311.78mg), the acoustic catalyst can be marked as "CZ-20", "CZ-30", "CZ-40", "CZ-50".

[0026] (II) Characterization of CdIn2S4 / ZnO composites

[0027] Figure 1 The XRD spectra of CdIn2S4 / ZnO composite materials with different composite ratios are shown in Figure 2. Figure 1It can be seen that the peak positions of the composite materials with different CdIn2S4 mass composite ratios are basically the same, and they contain most of the characteristic peaks of ZnO and CdIn2S4, with sharp peaks and basically no impurity peaks. This shows that the CdIn2S4 / ZnO composite materials synthesized with different CdIn2S4 mass ratios have high phase purity and high crystallinity. The reason why some of the characteristic peaks of ZnO do not appear may be because CdIn2S4 covers the surface of ZnO, and the reason why some of the characteristic peaks of CdIn2S4 do not appear may be because the content is too low.

[0028] Figure 2 The following are the scanning electron microscope (SEM) spectra of (A) ZnO, (B) CdIn2S4 and (C) CdIn2S4 / ZnO CZ-40 composite materials. Figure 2 It can be seen that ZnO is cubic and CdIn2S4 is flower ball-shaped. As can be seen from Figure C, after compounding CdIn2S4, some spherical substances are attached to the surface of CdIn2S4, indicating that the CZ-40 composite material was successfully prepared.

[0029] Example 2: Ultrasonic catalytic degradation of tetracycline hydrochloride by CdIn2S4 / ZnO composite material

[0030] (I) Method for removing tetracycline hydrochloride by stirring adsorption of CdIn2S4 / ZnO composite materials with different composite ratios:

[0031] Weigh 20 mg of CdIn2S4 / ZnO composite materials CZ-20, CZ-30, CZ-40, and CZ-50 with different composite ratios and pour them into a 250 mL conical flask, and add 20 ml of 50 mg / L tetracycline hydrochloride solution. Place the conical flask on a magnetic stirrer and stir for 30 minutes in the dark. After stirring, take a sample and centrifuge, take the supernatant, and use a UV-visible spectrophotometer to detect its absorbance near 375 nm, calculate the efficiency of CdIn2S4 / ZnO composite materials in adsorbing and removing tetracycline hydrochloride, and compare the reaction of adding CdIn2S4 / ZnO composite materials with different composite ratios to tetracycline hydrochloride solution.

[0032] (II) Method for the synergistic ultrasonic catalytic degradation of tetracycline hydrochloride by CdIn2S4 / ZnO composite materials with different composite ratios:

[0033] Weigh 20 mg of CdIn2S4 / ZnO composite materials CZ-20, CZ-30, CZ-40, CZ-50 with different composite ratios and pour them into a conical flask with a capacity of 250 mL, and add 20 ml of 50 mg / L tetracycline hydrochloride solution. Move the conical flask to a numerically controlled ultrasonic cleaner and ultrasonicate for 2 hours at 500 W. The ultrasonic process needs to be carried out under light-proof conditions. After the ultrasonication is completed, sample and centrifuge. After the same centrifugation, take the supernatant in a quartz cuvette and detect its absorbance near 375 nm with a UV-visible spectrophotometer. Calculate the efficiency of CdIn2S4 / ZnO composite materials in synergistic ultrasonic catalytic degradation of tetracycline hydrochloride, and compare the reaction of adding CdIn2S4 / ZnO composite materials with different composite ratios to tetracycline hydrochloride solution.

[0034] (III) Method for removing tetracycline hydrochloride by stirring and adsorption of CdIn2S4 / ZnO composite materials with different addition amounts:

[0035] In this experiment, CZ-40 was selected as the sonocatalyst, and the addition amount was 0.5g / L, 1g / L, 1.5g / L, 2g / L, and 3g / L respectively. The initial concentration of tetracycline hydrochloride was 30mg / L. 20mL was measured and added to a 250mL conical flask, and the conical flask was placed on a magnetic stirrer and stirred for 30min in the dark. After stirring, the sample was centrifuged, and the supernatant was taken for ultraviolet absorbance test, and the efficiency of removing tetracycline hydrochloride by stirring adsorption of different addition amounts of CdIn2S4 / ZnO composite material CZ-40 was calculated.

[0036] (IV) Method for the synergistic ultrasonic catalytic degradation of tetracycline hydrochloride by different addition amounts of CdIn2S4 / ZnO composite materials:

[0037] In this experiment, CZ-40 was selected as the sonocatalyst, and the addition amount was 0.5g / L, 1g / L, 1.5g / L, 2g / L, and 3g / L, respectively. The initial concentration of tetracycline hydrochloride was 30mg / L. 20mL was measured and added to a 250mL conical flask, and then placed in an ultrasonic cleaner. The ultrasonic time was 2h and the ultrasonic power was 500W. After the ultrasonic reaction, the mixed solution was sampled and centrifuged, and the supernatant was taken for ultraviolet absorbance test, and the efficiency of the synergistic ultrasonic catalytic degradation of tetracycline hydrochloride with different addition amounts of CdIn2S4 / ZnO composite material CZ-40 was calculated.

[0038] (V) Test results

[0039] Figure 3 This is a comparison chart of the efficiency of tetracycline hydrochloride adsorption removal and synergistic ultrasonic catalytic degradation by CdIn2S4 / ZnO composite materials with different composite ratios. Figure 3As shown, the adsorption removal rates of tetracycline hydrochloride by CdIn2S4, ZnO, CZ-20, CZ-30, CZ-40 and CZ-50 were 13.78(±2.19)%, 11.42(±0.83)%, 25.07(±2.93)%, 29.57(±3.00)%, 28.58(±3.39)% and 20.22(±1.97)%, respectively, and the ultrasonic degradation rates of tetracycline hydrochloride were 44.73(±7.69)%, 51.52(±6.72)%, 54.05(±5.52)%, 66.71(±5.42)%, 73.09(±1.04)% and 67.90(±3.72)%, respectively. It can be seen that the sonocatalytic performance of the prepared CdIn2S4 / ZnO composite materials is higher than that of pure CdIn2S4 and ZnO, indicating that the doping of CdIn2S4 is beneficial to improving the sonocatalytic activity of ZnO, and when the mass composite ratio of CdIn2S4 is 40%, that is, CZ-40, the removal rate of tetracycline hydrochloride is the highest.

[0040] Figure 4 The figure is a comparison of the efficiency of tetracycline hydrochloride adsorption and synergistic ultrasonic catalytic degradation by different amounts of CdIn2S4 / ZnO composite materials. Figure 4 As shown, the adsorption removal rates of tetracycline hydrochloride by CZ-40 with addition amounts of 0.5 g / L, 1 g / L, 1.5 g / L, 2 g / L, and 3 g / L were 23.84 (±2.39)%, 38.88 (±3.78)%, 48.56 (±2.03)%, 60.05 (±1.12)%, and 77.02 (±0.76)%, respectively. The ultrasonic degradation rates of tetracycline hydrochloride by CZ-40 at 0.5g / L, 1g / L, 1.5g / L, 2g / L and 3g / L were 30.76(±2.48)%, 67.36(±3.89)%, 84.72(±3.63)%, 91.03(±1.41)%, 92.42(±0.73)% and 96.43(±0.12)% respectively. It can be seen that with the increase of the amount of catalyst added, the adsorption removal rate and ultrasonic degradation rate of tetracycline hydrochloride also gradually increased. However, when the amount added increased to 1.5g / L, the degradation rate reached 91.03(±1.41)%. After that, when the amount added increased further, the increasing trend of the ultrasonic degradation rate became less obvious, which may be due to the excessive catalyst, which produced a masking effect on ultrasound.

Claims

1. A CdIn 2 S 4 / ZnO composite materials, It is characterized in that The CdIn 2 S 4 / ZnO composites, CdIn 2 S 4 The mass ratio of ZnO is 20%-50%.

2. The CdIn according to claim 1 2 S 4 / ZnO composite materials, It is characterized in that ZnO, Cd(NO 3 ) 2 ·4H 2 O, TAA and InCl 3 ·4H 2 O was dissolved in deionized water and stirred to perform a hydrothermal reaction. The precipitate obtained by the reaction was washed three times with deionized water and anhydrous ethanol respectively, and then the product was dried to obtain CdIn 2 S 4 / ZnO composite materials.

3. A CdIn according to claim 2 2 S 4 Preparation method of ZnO composite material, It is characterized in that Cd(NO 3 ) 2 ·4H 2 O, TAA and InCl 3 ·4H 2 The molar ratio of O is 0.65:4.46:

1.

4. A CdIn according to claim 2 2 S 4 Preparation method of ZnO composite material, It is characterized in that The hydrothermal reaction conditions are 180°C for 16 h.

5. A CdIn according to claim 2 2 S 4 Preparation method of ZnO composite material, It is characterized in that The drying temperature is 80°C and the drying time is 16 hours.

6. The CdIn according to claim 1 2 S 4 Application of ZnO / ZnO composite materials in ultrasonic catalytic degradation of organic pollutants in wastewater.

7. A CdIn according to claim 6 2 S 4 Application of / ZnO composite materials in ultrasonic catalytic degradation of organic pollutants in wastewater, It is characterized in that The steps are as follows: Add CdIn to wastewater containing organic pollutants 2 S 4 / ZnO composite materials and ultrasonicated them at an ultrasonic power of 500 W for 2 h.

8. A CdIn according to claim 7 2 S 4 Application of / ZnO composite materials in ultrasonic catalytic degradation of organic pollutants in wastewater, It is characterized in that The initial concentration of organic pollutants was 30 mg / L.

9. A CdIn according to claim 7 2 S 4 Application of / ZnO composite materials in ultrasonic catalytic degradation of organic pollutants in wastewater, It is characterized in that The organic pollutant is tetracycline hydrochloride.

10. A CdIn according to claim 7 2 S 4 Application of / ZnO composite materials in ultrasonic catalytic degradation of organic pollutants in wastewater, It is characterized in that CdIn 2 S 4 The addition amount of / ZnO composite materials was 0-3g / L respectively.

Citation Information

Patent Citations

  • Preparation method and application of ZnO-loaded CdIn2S4 nano-cube composite catalyst

    CN107262115A

  • Preparation method and application of composite catalyst

    CN114308073A

  • Application of heterojunction CdIn2S4 / Bi2WO6 piezoelectric-optical composite catalyst in piezoelectric optical degradation of organic matters

    CN115400768A

  • UiO66 / ZnO composite material and preparation method and application thereof

    CN116440957A