Core-shell type manganese-based diatomic catalyst as well as preparation method and application thereof

By preparing a core-shell manganese-based diatomic catalyst, the problems of high temperature, low efficiency, and poor stability of existing catalysts in formaldehyde degradation reactions are solved, and efficient, safe, and economical formaldehyde removal effects are achieved.

CN118719115APending Publication Date: 2024-10-01JIEYANG QINGCHEN TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410774003.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing catalysts have problems such as high temperature, low degradation efficiency, and poor stability in formaldehyde degradation reactions, especially at room temperature/near room temperature. It is necessary to develop more efficient and gentle non-noble metal catalysts.

Method used

Using the preparation method of core-shell manganese-based diatomic catalyst, the rhombic dodecahedral manganese-based bimetallic organic framework is coated with multi-layer silica to achieve atomic level dispersion of metal elements to form Mn/N-C@B/ SiO2 catalyst for formaldehyde degradation reaction.

Benefits of technology

It has achieved a formaldehyde removal rate of more than 99%, has good stability, degrades at low temperature and low pressure, has high safety, and has low metal content and has a cost advantage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719115A_ABST
    Figure CN118719115A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts for catalyzing formaldehyde degradation, and particularly discloses a core-shell type manganese-based double-atom catalyst and a preparation method and application thereof.A rhombic dodecahedron manganese-based double-metal organic framework is prepared, and metal Mn exists in an atomic-scale dispersion form; the other metal element is one of Fe, Co, Ni, Cu, Ag, Pt, Pd and Rh and exists in the atomic-scale dispersion form; the surface of the catalyst is coated with multiple layers of silicon dioxide, controllable preparation of the Mn / N-C-B / SiO2 core-shell type manganese-based diatomic catalyst is achieved, and the catalyst shows excellent activity in formaldehyde degradation reaction and is easy to prepare, small in pollution and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts for catalyzing formaldehyde degradation, in particular to a core-shell manganese-based diatomic catalyst and a preparation method and application thereof. Background Art

[0002] Formaldehyde (HCHO) is one of the main volatile organic compounds in indoor air. It has a significant impact on indoor air quality and thus affects human health. Long-term exposure to HCHO is harmful to human health and can cause headaches, pneumonia, and lung cancer. Among the methods of removing HCHO, catalytic oxidation is the conversion of HCHO into non-toxic products (such as CO 2 and H 2 O) is a prominent method. Precious metal-based catalysts (Pt, Au and Pd) show excellent catalytic performance for HCHO oxidation at room temperature, but considering the limited reserves and economy of precious metals, the development of efficient and stable non-precious metal formaldehyde degradation catalysts is of great significance in both basic research and industrial applications. In recent years, researchers have developed a variety of catalysts for formaldehyde degradation reactions, including single-atom catalysts, alloy catalysts, non-precious metal catalysts, etc., which have achieved good catalytic performance in formaldehyde degradation reactions. For example, 202410041616.7 discloses a room-temperature catalytic formaldehyde decomposition material based on a metal-organic framework and a preparation method thereof, wherein the room-temperature catalytic formaldehyde decomposition material based on a metal-organic framework includes a manganese salt and an organic ligand, wherein the manganese salt is one of manganese sulfate or manganese nitrate, and the organic ligand is an organic ligand containing a benzene ring and a carboxyl group. 201910865957.5 discloses a catalyst for photocatalytic degradation of formaldehyde, its preparation method and use, and the general formula of the catalyst for photocatalytic degradation of formaldehyde is MOx / TiO 2 , wherein M includes any one of Fe, Ni, Cu, Co or Mn or a combination of at least two thereof, x is the amount of oxygen required to satisfy the valence balance, TiO 2 It has a rutile structure.

[0003] However, the above catalysts have problems such as high formaldehyde degradation temperature, low degradation efficiency, and poor stability when used in formaldehyde degradation reactions. Therefore, for formaldehyde degradation reactions at room temperature or near room temperature, non-precious metal catalysts with better reaction performance and milder reaction conditions are needed. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a core-shell manganese-based diatomic catalyst and a preparation method and application thereof.

[0005] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0006] One of the purposes of the present invention is to provide a method for preparing a core-shell manganese-based diatomic catalyst, comprising the following steps:

[0007] S1, take the first metal precursor, Zn(NO 3 ) 2 6H 2 O, 2-methylimidazole were added to excess methanol, stirred at room temperature for 1-6 hours, and then centrifuged, washed, and dried to obtain A-ZIF-8;

[0008] S2, taking a second metal B precursor and Mn-ZIF-8 in a mass ratio of 1:(1-1000), adding the second metal B precursor to tetraethyl silicate and deionized water in a volume ratio of 1:(2.5-20), and mixing them evenly to obtain a second metal B precursor mixed solution;

[0009] S3, dispersing Mn-ZIF-8 in ethanol, adjusting the pH to 8-11, and adding the second metal B precursor mixed solution in multiple times, stirring for 18 hours, and obtaining a solid sample after centrifugation, washing, and drying;

[0010] S4, calcining the obtained solid sample to obtain the core-shell diatomic catalyst A / NC@B / SiO 2 .

[0011] Furthermore, the first metal A precursor is Mn(NO 3 ) 2 ·4H 2 O.

[0012] Furthermore, the second metal B precursor is a nitrate or chloride of one of Fe, Co, Ni, Cu, Ag, Pt, Pd, and Rh.

[0013] Preferably, in step S1, methanol is used for washing three times, and then dried at 40-80° C. overnight.

[0014] Preferably, in step S3, aqueous ammonia is used to adjust the pH.

[0015] Preferably, in step S3, the second metal B precursor mixed solution is added in 2-10 times, with an interval of 10-30 minutes between each addition.

[0016] Preferably, in step S3, washing is performed with ethanol for 3 times, followed by drying at 40-80° C. overnight.

[0017] Specifically, step S4 is as follows: heating the solid sample from room temperature to 800-1100°C at a heating rate of 5°C / min under a nitrogen atmosphere and keeping the temperature for 2 hours, cooling the temperature to room temperature to obtain the core-shell diatomic catalyst A / NC@B / SiO 2 .

[0018] The second object of the present invention is to provide a core-shell manganese-based diatomic catalyst prepared by the above method.

[0019] The third object of the present invention is to provide a core-shell manganese-based diatomic catalyst for use in catalyzing formaldehyde degradation.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention prepares a rhombic dodecahedral manganese-based bimetallic organic framework, wherein the metal Mn exists in an atomically dispersed form; another metal element is one of Fe, Co, Ni, Cu, Ag, Pt, Pd, and Rh, which also exists in an atomically dispersed form; and then multilayer silicon dioxide is coated on the surface to achieve Mn / NC@B / SiO 2 The controllable preparation of core-shell manganese-based diatomic catalysts shows excellent activity in formaldehyde degradation reaction, is simple to prepare, has low pollution and is environmentally friendly;

[0022] (2) Mn / NC@B / SiO prepared by the present invention 2 The core-shell manganese-based diatomic catalyst is used in the formaldehyde degradation reaction, achieving efficient utilization of active components; the formaldehyde removal rate can reach more than 99% with good stability;

[0023] (3) Mn / NC@B / SiO prepared by the present invention 2 The core-shell manganese-based diatomic catalyst is used in the formaldehyde degradation reaction, achieving formaldehyde degradation at low temperature and low pressure, with high safety and good economic benefits;

[0024] (4) Mn / NC@B / SiO prepared by the present invention 2 The core-shell manganese-based diatomic catalyst has a low metal content under the same benefit. The added second metal can greatly improve the formaldehyde removal rate and has certain cost advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The core-shell manganese-based diatomic catalyst sample is Mn / NC@Fe / SiO 2 XRD pattern of .

[0026] Figure 2 The core-shell manganese-based diatomic catalyst sample is Mn / NC@Fe / SiO 2Transmission electron microscopy image of .

[0027] Figure 3 The core-shell manganese-based diatomic catalyst sample is Mn / NC@Fe / SiO 2 Formaldehyde removal (conversion) rate.

[0028] Figure 4 The core-shell manganese-based diatomic catalyst sample Mn / NC@Cu / SiO 2 XRD pattern of .

[0029] Figure 5 The core-shell manganese-based diatomic catalyst sample Mn / NC@Cu / SiO 2 Transmission electron microscopy image of .

[0030] Figure 6 The core-shell manganese-based diatomic catalyst sample Mn / NC@Cu / SiO 2 Formaldehyde removal (conversion) rate. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.

[0032] Unless otherwise specified, the raw materials and reagents used in the following examples were commercially available or prepared by known techniques.

[0033] Example 1

[0034] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol for 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.15 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then a second metal B precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 42 mg Fe(NO 3 ) 3 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, a core-shell diatomic catalyst sample, Mn / NC@Fe / SiO 2 .

[0035] Figure 1 The core-shell diatomic catalyst sample is Mn / NC@Fe / SiO 2 XRD pattern of Figure 2 The core-shell diatomic catalyst sample is Mn / NC@Fe / SiO 2 TEM image of Figure 1 , Figure 2 It can be seen that no nanoparticles were observed, and both Mn and Fe were in atomic-level dispersion, indicating that the core-shell diatomic catalyst sample Mn / NC@Fe / SiO 2 Successful preparation.

[0036] Example 2

[0037] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.3 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 24 mg Fe(NO 3 ) 3 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling down to room temperature, the core-shell diatomic catalyst sample Mn / NC@Fe / SiO was obtained. 2 .

[0038] Example 3

[0039] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol for 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.3 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 42 mg Fe(NO 3 ) 3 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, the core-shell diatomic catalyst sample Mn / NC@Fe / SiO was obtained. 2 .

[0040] Example 4

[0041] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol for 3 times, and finally dried at 60 °C overnight to obtain Mn-ZIF-8; then 0.15 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 64 mg Fe(NO 3 ) 3 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, the core-shell diatomic catalyst sample Mn / NC@Fe / SiO 2 .

[0042] Example 5

[0043] Weigh 0.5 g Mn(NO 3 ) 2 ·4H2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.15 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 34 mg Cu(NO 3 ) 2 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, the core-shell diatomic catalyst sample Mn / NC@Cu / SiO was obtained. 2 ; Figure 4 Core-shell diatomic catalyst sample Mn / NC@Cu / SiO 2 XRD pattern of Figure 5 Core-shell diatomic catalyst sample Mn / NC@Cu / SiO 2 Transmission electron microscopy image of .

[0044] Example 6

[0045] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.15 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 34 mg Ni(NO 3 ) 2 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, the core-shell diatomic catalyst sample Mn / NC@Ni / SiO 2 .

[0046] Example 7

[0047] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol for 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.15 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 30 mg Co(NO 3 ) 2 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling down to room temperature, the core-shell diatomic catalyst sample Mn / NC@Co / SiO was obtained. 2 .

[0048] Example 8

[0049] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3 g 2-methylimidazole were added to a beaker containing 200 mL methanol, stirred at 500 r / min for 3 h at room temperature, centrifuged, washed with methanol 3 times, and finally dried at 60 ° C overnight to obtain Mn-ZIF-8; then 0.15 g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50 mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then the second metal precursor mixed solution (1 mL tetraethyl silicate, 8 mL deionized water, 64 mg [Pt(NH 3 ) 4 ](NO 3 )2 The sample was added in 3 times, 30 minutes each time, and finally stirred for 18 hours, centrifuged, washed, and dried at 60°C overnight; the sample obtained above was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, the core-shell diatomic catalyst sample Mn / NC@Pt / SiO 2 .

[0050] Comparative Example

[0051] Weigh 0.5 g Mn(NO 3 ) 2 ·4H 2 O, 0.6 g Zn(NO 3 ) 2 6H 2 O and 2.3g 2-methylimidazole were added to a beaker containing 200mL methanol, stirred at 500r / min for 3h at room temperature, centrifuged, washed with methanol for 3 times, and finally dried at 60°C overnight to obtain Mn-ZIF-8; then 0.15g of the obtained Mn-ZIF-8 sample was weighed and added to a beaker containing 50mL ethanol, ultrasonically dispersed, and then an appropriate amount of ammonia water was added to adjust the pH to 8-9, and then 1mL tetraethyl silicate and 8mL deionized water were added in 3 times, 30min each time, and finally stirred for 18h, centrifuged, washed, and dried at 60°C overnight; the above-obtained sample was placed in a tube furnace N 2 The temperature was raised from room temperature to 900 °C at a rate of 5 °C / min under an atmosphere and kept at this temperature for 2 hours. After cooling to room temperature, the core-shell single atom catalyst sample Mn / NC@SiO 2 .

[0052] Application Examples

[0053] The catalytic HCHO degradation activity was evaluated in a fixed bed reactor. 100 mg of the core-shell diatomic catalyst sample, Mn / NC@Fe / SiO 2 , core-shell diatomic catalyst sample 2 Mn / NC@Fe / SiO 2 , core-shell diatomic catalyst sample three Mn / NC@Fe / SiO 2 , core-shell diatomic catalyst sample 4 Mn / NC@Fe / SiO 2 , Core-shell diatomic catalyst sample 5 Mn / NC@Cu / SiO 2 , core-shell diatomic catalyst sample VI Mn / NC@Ni / SiO 2 , core-shell diatomic catalyst sample 7 Mn / NC@Co / SiO 2, core-shell diatomic catalyst sample 8 Mn / NC@Pt / SiO 2 , Core-shell single atom catalyst sample 9 Mn / NC@ / SiO 2 , air was bubbled into an aqueous solution containing 4 wt % formaldehyde at a flow rate of 60 mL / min under normal pressure to produce a formaldehyde concentration of 100 ppm, and the reaction was carried out at 25°C for 100 h; the formaldehyde content was determined by an ultraviolet spectrophotometer, and the formaldehyde removal rate was calculated by comparing the formaldehyde content before and after the reaction. The test results are shown in Table 1.

[0054] Table 1

[0055] Catalyst samples Formaldehyde removal rate% Catalyst sample 1 95.7 Catalyst sample 2 98.6 Catalyst sample 3 96.7 Catalyst sample 4 99.5 Catalyst sample 5 95.9 Catalyst sample 6 98.1 Catalyst sample 7 97.6 Catalyst sample eight 96.2 Catalyst sample nine 78.5

[0056] As can be seen from Table 1, when the core-shell manganese-based diatomic catalyst prepared by the present invention catalyzes HCHO to degrade formaldehyde, the formaldehyde removal rate is above 95%, and can reach up to above 99%.

[0057] Furthermore, the above method was used again to test the stability of the catalyst after catalyzing HCHO degradation for 300 hours. The test results are shown in Table 2.

[0058] Table 2

[0059] Catalyst samples Formaldehyde removal rate% Catalyst sample 1 90.4 Catalyst sample 2 95.7 Catalyst sample 3 91.5 Catalyst sample 4 98.4 Catalyst sample 5 90.2 Catalyst sample 6 95.4 Catalyst sample 7 93.6 Catalyst sample eight 91.2 Catalyst sample nine 60.9

[0060] It can be seen from Table 2 that after 300 hours, the formaldehyde removal rate is still above 90%, indicating that the core-shell manganese-based diatomic catalyst prepared by the present invention has high stability.

[0061] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A method for preparing a core-shell manganese-based diatomic catalyst, characterized in that: The following steps are involved: S1. Add the first metal precursor, Zn(NO3)2·6H2O, and 2-methylimidazole in a mass ratio of (1-10):(1-20):(4-80) to an excess of methanol, stir at room temperature for 1-6 hours, centrifuge, wash, and dry to obtain A-ZIF-8; S2, taking a second metal B precursor and Mn-ZIF-8 in a mass ratio of 1:(1-1000), adding the second metal B precursor to tetraethyl silicate and deionized water in a volume ratio of 1:(2.5-20), and mixing them evenly to obtain a second metal B precursor mixed solution; S3, dispersing Mn-ZIF-8 in ethanol, adjusting the pH to 8-11, and adding the second metal B precursor mixed solution in multiple times, stirring for 18 hours, and obtaining a solid sample after centrifugation, washing, and drying; S4. The solid sample is calcined to obtain a core-shell diatomic catalyst A / NC@B / SiO2.

2. The method for preparing the core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: The first metal A precursor is Mn(NO3)2·4H2O.

3. The method for preparing the core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: The second metal B precursor is a nitrate or chloride of one of Fe, Co, Ni, Cu, Ag, Pt, Pd, and Rh.

4. The method for preparing the core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: In the step S1, methanol is used for washing three times, and then dried at 40-80° C. overnight.

5. The method for preparing the core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: In step S3, ammonia water is used to adjust the pH.

6. The method for preparing the core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: In step S3, the second metal B precursor mixed solution is added in 2-10 times, with an interval of 10-30 minutes between each addition.

7. The method for preparing the core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: In the step S3, washing is performed with ethanol for 3 times, and then drying is performed at 40-80° C. overnight.

8. The method for preparing a core-shell manganese-based diatomic catalyst according to claim 1, characterized in that: The step S4 is specifically as follows: heating the solid sample from room temperature to 800-1100°C at a heating rate of 5°C / min under a nitrogen atmosphere and keeping the temperature for 2 hours, and then cooling the temperature to room temperature to obtain the core-shell diatomic catalyst A / NC@B / SiO2.

9. A core-shell manganese-based diatomic catalyst prepared by the method according to any one of claims 1 to 8.

10. Use of the core-shell manganese-based diatomic catalyst as claimed in claim 9 in catalyzing formaldehyde degradation.

Citation Information

Patent Citations

  • Preparation method of MOx@SiO2 shell-core structure catalyst

    CN103418371A

  • Two dimensional catalytic material derived from metal-organic frameworks and application thereof in removal of volatile organic compounds (VOCs)

    CN110787788A

  • Preparation method of MOF derived hollow cobalt oxide loaded manganese oxide catalyst as well as product and application thereof

    CN112569961A

  • Formaldehyde adsorbent

    CN112619607A

  • Monatomic catalyst based on functionalized MOF (Metal Organic Framework) as well as preparation method and application of monatomic catalyst

    CN116130686A