High-activity bifunctional catalytic material as well as preparation method and application thereof

By constructing palladium-tungsten oxide bifunctional active sites on a two-dimensional alumina support, the problem of single active site and insufficient deep oxidation ability of palladium-based catalytic materials has been solved, and efficient methyl ethyl ketone purification has been achieved, which has important application prospects.

CN118719167AActive Publication Date: 2024-10-01XI AN JIAOTONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410812237.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing palladium-based catalytic materials have a single active site and insufficient deep oxidation capabilities, which limits their industrial application in the field of volatile organic pollutant purification.

Method used

A method for preparing highly active bifunctional catalytic materials is adopted, by reacting aluminum nitrate nonahydrate with urea in deionized water, adding surfactant and ethanol, crystallizing and roasting to form an alumina carrier, and then reacting with metatungstic acid The ammonium and palladium salt solutions react to introduce tungsten oxide and palladium clusters to form palladium-tungsten oxide bifunctional active sites on the two-dimensional alumina support.

Benefits of technology

It significantly improves the low-temperature catalytic efficiency and reaction stability of catalytic materials, can effectively purify methyl ethyl ketone at 40-260°C, and solves the problems of single active site and insufficient deep oxidation ability of palladium-based catalytic materials, which is of great importance. application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719167A_ABST
    Figure CN118719167A_ABST
Patent Text Reader

Abstract

The invention discloses a high-activity bifunctional catalytic material and a preparation method and application thereof.The preparation method comprises the steps that aluminum nitrate and urea are dissolved in water, ethyl alcohol and a surfactant are added, and primary roasting is performed after crystallization to obtain primary roasting powder; adding the primary roasting powder into an ammonium metatungstate solution, uniformly mixing, carrying out rotary evaporation to obtain a solid, and carrying out secondary roasting on the solid to obtain final powder; and uniformly adding the final powder into water, adding a palladium salt solution for loading, and then roasting for three times to obtain the high-activity bifunctional catalytic material. According to the invention, a palladium-atomic-scale dispersed tungsten oxide-double active site high-activity bifunctional catalytic material is constructed through a two-step method, and the problem that methyl ethyl ketone cannot be deeply mineralized by a pure palladium catalyst at a low temperature is solved. Due to the palladium-tungsten synergistic effect of the prepared high-activity bifunctional catalytic material, the high-activity bifunctional catalytic material has excellent low-temperature deep oxidation activity and reaction stability of methyl ethyl ketone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of air pollution control, and particularly relates to a high-activity dual-functional catalytic material and a preparation method and application thereof. Background Art

[0002] Volatile Organic Compounds (VOCs) refer to organic compounds with a boiling point below 260°C at atmospheric pressure (250.101 kpa), or organic compounds with a saturated vapor pressure exceeding 133.32 Pa at room temperature (25°C) and emitted into the air in the form of gaseous molecules. There are many types of VOCs, mainly including aliphatic hydrocarbons, oxygenated hydrocarbons, aromatic hydrocarbons and their derivatives, halogenated hydrocarbons, nitrogen-containing hydrocarbons, sulfur-containing hydrocarbons, etc., which can be divided into outdoor sources and indoor sources. The reason why oxygenated volatile organic compounds (OVOCs, such as formaldehyde, acetone, methyl ethyl ketone, ethyl acetate, etc.) are worrying is that they are very easy to form ozone, causing photochemical smog, urban haze and other air pollution problems, and they also have great harm to the functions of the human immune system, kidneys and respiratory system, and are highly toxic and carcinogenic. Among them, methyl ethyl ketone (MEK) is a typical OVOCs, which are widely used as solvents in many large-scale processes (such as printing and manufacturing). Therefore, developing an efficient strategy for removing methyl ethyl ketone is of great significance for controlling VOCs.

[0003] Complete catalytic oxidation is a promising method for treating volatile organic compounds, especially low concentrations (<0.5 vol.%), into carbon dioxide and water. The development of efficient and promising low-temperature VOCs reduction catalysts continues to attract widespread attention. Supported precious metal catalysts are widely used in the removal of oxygenated hydrocarbons due to their good activity and strong regeneration ability. However, the further industrial application of pure palladium-based catalysts is limited by factors such as the single active site and insufficient deep oxidation ability. Summary of the invention

[0004] In order to overcome the problems of single active site and insufficient deep oxidation ability of palladium-based catalytic materials in the prior art, the purpose of the present invention is to provide a high-activity bifunctional catalytic material and a preparation method and application. The catalytic material prepared by this method has good deep oxidation ability and reaction stability of methyl ethyl ketone, and has important application prospects in the field of low-temperature purification of volatile organic pollutants.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a highly active bifunctional catalytic material comprises the following steps:

[0007] Aluminum nitrate nonahydrate and urea are dissolved in deionized water, ethanol and a surfactant are added, and then crystallization is performed, centrifugation, washing, drying, and then calcination is performed once to obtain a calcined powder;

[0008] The primary calcined powder is added to the ammonium metatungstate solution, and after stirring and reacting completely, a solid is obtained by rotary evaporation, and the solid is subjected to secondary calcination to obtain the final powder;

[0009] The final powder is added to water to obtain a tungsten oxide-alumina carrier suspension, the pH is adjusted to 6-11, and then a palladium salt solution is added, and the reaction is carried out at 90-110°C for 1-2 hours to obtain a light yellow solid;

[0010] The light yellow solid was calcined three times to obtain a highly active bifunctional catalytic material.

[0011] Furthermore, the molar ratio of aluminum nitrate nonahydrate to urea is 3-6:6-12 mmoL.

[0012] Furthermore, the surfactant is dodecylamine.

[0013] Further, the ratio of aluminum nitrate nonahydrate to ethanol is 3-6 mmol: 8-12 mL;

[0014] The usage ratio of aluminum nitrate nonahydrate to surfactant is 3-6mmol:0.25-0.5g.

[0015] Further, the crystallization temperature is 150-170°C and the time is 3-5h;

[0016] The primary calcination temperature is 550-650°C for 4-6 hours; the temperature is increased to 550-650°C at a heating rate of 2-5°C / min.

[0017] Further, the mass ratio of the primary calcined powder to ammonium metatungstate is 0.5 g 0.00275-0.11 g;

[0018] The secondary calcination temperature is 600-650°C, and the time is 4-6h; the temperature is increased to 600-650°C at a heating rate of 2-5°C / min.

[0019] Further, the final powder and palladium salt solution dosage ratio is 0.2 g:5 mL, and the concentration of the palladium salt solution is 0.00015-0.0006 g / mL;

[0020] The palladium salt is palladium nitrate, palladium chloride or sodium tetrachloropalladate.

[0021] Furthermore, the temperature of the three calcinations is 200-300° C., and the time is 1-1.5 h; the three calcinations are performed under a mixture of hydrogen and argon;

[0022] The volume percentage of hydrogen in the mixture of hydrogen and argon is 5-10%;

[0023] The flow rate of the mixture of hydrogen and argon is 100-200 mL / min.

[0024] A highly active bifunctional catalytic material, wherein the specific surface area of ​​the catalytic material is 159.0-170.9 m 2 / g, micropore volume is 0.067-0.071cm 3 / g.

[0025] The invention discloses an application of a highly active bifunctional catalytic material in the purification of volatile oxygen-containing hydrocarbons.

[0026] Furthermore, the highly active bifunctional catalytic material is heated at 40-260°C and a space velocity of 30,000-45,000 h -1 , under the condition of oxygen volume concentration of 10-21%, the purification of methyl ethyl ketone with a volume concentration of 0.6% is achieved.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] In the present invention, a surfactant is added to the aluminum nitrate and urea solution to increase the complexing degree of the γ-AlOOH precursor and increase the pore volume and specific surface area of ​​the two-dimensional layered alumina carrier, which is beneficial to the adsorption of pollutant molecules and the dispersion of active metals, thereby improving the reaction performance of the catalyst. And an atomically dispersed tungsten oxide is introduced on the surface of the alumina carrier using a one-step method. In the present invention, the pH is adjusted to 6-11 to further promote the formation of highly stable palladium clusters. The strong interaction between the active phase of the palladium cluster and the atomically dispersed tungsten oxide accelerates the charge balance process between the carrier and the noble metal, greatly improving the low-temperature catalytic efficiency and reaction stability of the bifunctional catalytic material. In the present invention, a special bifunctional active site of palladium-tungsten oxide on a two-dimensional alumina carrier is successfully constructed by a simple two-step method, which solves the problem of expensive cost of supported noble metals to a certain extent, overcomes the defects of the existing single palladium-based catalytic materials with a single active site and insufficient deep oxidation ability, and has the prospect of universal application.

[0029] The specific surface area of ​​the high-activity bifunctional catalytic material prepared by the present invention is 159.0-170.9m 2 / g, micropore volume is 0.067-0.071cm 3 / g, has a large specific surface area, which is beneficial to improving the catalytic efficiency.

[0030] The high-activity bifunctional catalytic material prepared by the present invention can be used in the purification of volatile oxygen-containing hydrocarbons. -1Under the condition of oxygen volume concentration of 10-20%, purification of methyl ethyl ketone with a volume concentration of 0.6% is achieved; the prepared catalytic material of the present invention has good methyl ethyl ketone deep oxidation ability and reaction stability, and has important application prospects in the field of low-temperature purification of volatile organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The HADDF images of the high-activity bifunctional catalytic material of the present invention under a transmission electron microscope; wherein: (a) is a low magnification, (b) is a medium magnification, and (c) is a high magnification;

[0032] Figure 2 These are EDS-mapping images of the highly active bifunctional catalytic material of the present invention; wherein (a) is a low-magnification image of HADDF, (b) is the EDS of tungsten (W), and (c) is the EDS of palladium (Pd);

[0033] Figure 3 This is the XRD spectrum of the highly active bifunctional catalytic material of the present invention;

[0034] Figure 4 The purification efficiency curve of the high-activity bifunctional catalytic material of the present invention for methyl ethyl ketone;

[0035] Figure 5 for Figure 4 The corresponding CO2 generation rate curve;

[0036] Figure 6 It is a cyclic stability test of the highly active bifunctional catalytic material of the present invention;

[0037] Figure 7 This is the efficiency curve of the long-term stability test of the high-activity bifunctional catalytic material in the present invention for methyl ethyl ketone purification. DETAILED DESCRIPTION

[0038] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. The present invention will be described in detail below in conjunction with the embodiments.

[0039] In the present invention, the complexing degree of the γ-AlOOH precursor is increased by adding a surfactant to the aluminum nitrate and urea solution, and the pore volume and specific surface area of ​​the two-dimensional layered alumina carrier are increased, which is beneficial to the adsorption of pollutant molecules and the dispersion of active metals, thereby improving the reaction performance of the catalyst. And by a simple impregnation-rotary evaporation drying method, atomically dispersed tungsten oxide is introduced on the surface of the alumina carrier. In the present invention, the pH of the tungsten oxide-alumina carrier suspension is adjusted to further promote the formation of highly stable palladium clusters, and then the strong interaction between the active phase of the palladium cluster and the atomically dispersed tungsten oxide accelerates the charge balance process between the carrier and the noble metal, greatly improving the low-temperature catalytic efficiency and reaction stability of the bifunctional catalytic material. In the present invention, a special bifunctional active site of palladium-tungsten oxide on a two-dimensional alumina carrier is successfully constructed through a two-step ligand thermal decomposition method of the synthesis method, which solves the problem of expensive cost of supported noble metals to a certain extent, overcomes the defects of the existing single palladium-based catalytic materials with a single active site and insufficient deep oxidation ability, and has the prospect of universal application.

[0040] A method for preparing a highly active bifunctional catalytic material of the present invention is as follows:

[0041] Dissolve aluminum nitrate nonahydrate and urea in deionized water and stir vigorously to mix evenly. Then slowly drip ethanol, add surfactant, and stir vigorously. Crystallize the mixed solution in a reactor, centrifuge and wash several times, dry to obtain a white precipitate, and roast once to obtain a solid powder. Dissolve ammonium metatungstate in deionized water and stir evenly, add solid powder, and perform rotary evaporation after the reaction is complete. The obtained powder is roasted twice to obtain the final powder.

[0042] The final powder obtained above is dispersed in water, stirred evenly, the pH is adjusted to 6-11, and then heated to a certain temperature after stirring evenly, and stirred continuously, and a dihydrated palladium nitrate aqueous solution is added dropwise to form a light yellow transparent solution. After the reaction is complete, centrifugation, washing, and vacuum drying are performed, and the yellow-brown powder is calcined in a hydrogen and argon atmosphere to obtain a highly active bifunctional catalytic material.

[0043] Specifically, the preparation method of the high-activity bifunctional catalytic material of the present invention comprises the following steps:

[0044] (1) dissolving 3-6 mmoL aluminum nitrate nonahydrate and 6-12 mmoL urea in 65-75 mL of deionized water, and stirring at 400-600 rpm for 10-30 min to uniformly disperse the mixture to obtain a transparent solution;

[0045] (2) adding 8-12 mL of ethanol dropwise to the transparent solution obtained in step (1), followed by adding 0.25-0.5 g of a surfactant (dodecylamine), and stirring at 400-600 rpm for 30-60 min to uniformly disperse the mixture to obtain a transparent mixed solution;

[0046] (3) placing the transparent mixed solution obtained in step (2) in a hydrothermal reactor for crystallization to generate γ-AlOOH, the crystallization temperature is 150-170° C., the time is 3-5 hours, and a milky white suspension is obtained;

[0047] (4) centrifuging the milky white suspension obtained in step (3) at a speed of 6000-10000 rpm, washing with a mixed solution of ethanol: deionized water in a volume ratio of 1:1-1.5, and drying at 80-120° C. to obtain a white solid powder;

[0048] (5) The white solid powder obtained in step (4) is calcined once in an air atmosphere to convert γ-AlOOH into alumina at a temperature of 550-650° C. for 4-6 h at a heating rate of 2-5° C. / min to obtain a powder.

[0049] (6) Dissolve 0.00275-0.11 g of ammonium metatungstate in 50 mL of water to make it evenly dispersed, add 0.5 g of the powder obtained by the first calcination in step (5), stir at a speed of 400-800 rpm for 2-6 h, and the rotary evaporation temperature is 50-70° C. and the speed is 120-140 r / min.

[0050] (7) The powder obtained by rotary evaporation in step (6) is subjected to secondary calcination in an air atmosphere to generate tungsten oxide at a temperature of 600-650° C. for 4-6 h at a heating rate of 2-5° C. / min to obtain a final powder.

[0051] (7) 0.2 g of the final powder obtained by the secondary calcination in step (6) is placed in 45-50 mL of deionized water to make it evenly dispersed, and the pH is adjusted to 6-11 with 0.25 mol / L anhydrous sodium carbonate solution, and stirring is continued to make it uniform.

[0052] (8) The solution in step (7) was heated to 90-110° C., 5 mL of a 0.00015-0.0008 g / mL aqueous solution of palladium nitrate (palladium chloride or sodium tetrachloropalladate) was added dropwise, and stirring was continued at 600-800 rpm for 1-2 h.

[0053] (9) After the solution obtained in step (8) cools to room temperature, centrifuge at 6000-9000 rpm, wash with deionized water 5 times, and vacuum dry at 50-70° C. to obtain a light yellow solid powder;

[0054] (10) calcining the light yellow solid powder obtained in step (9) in a mixed atmosphere of hydrogen and argon, wherein the flow rate of the mixed gas of hydrogen and argon is 100-200 mL / min, the temperature is 200-300° C., and the time is 1-1.5 h to obtain a high-activity bifunctional catalytic material. The volume percentage of hydrogen in the mixed gas of hydrogen and argon is 5-10%.

[0055] The high-activity bifunctional catalytic material prepared by the present invention has two active sites, palladium clusters and atomic-level dispersed tungsten oxide, and has a high specific surface area (159.0-170.9m 2 / g) and micropore volume (0.067-0.071cm 3 / g).

[0056] The high-activity bifunctional catalytic material prepared by the present invention can be used in the purification of volatile oxygen-containing hydrocarbons. Specifically, 40-260°C, space velocity 30000-45000h -1 Under the condition of oxygen volume concentration of 10-20%, purification of methyl ethyl ketone with a volume concentration of 0.6% is achieved; the prepared catalytic material of the present invention has good low-temperature deep oxidation ability and anti-chlorine stability.

[0057] The following are specific embodiments.

[0058] Example 1 Preparation of aluminum oxide (Al2O3) by hydrothermal method

[0059] (1) Dissolve 3 mmol of aluminum nitrate nonahydrate and 6 mmol of urea in 70 mL of deionized water and stir at 600 rpm for 10 min to make them evenly dispersed;

[0060] (2) adding 10 mL of ethanol dropwise to the transparent solution obtained in step (1), followed by adding a surfactant such as dodecylamine, and stirring at 500 rpm for 30 min to uniformly disperse the solution;

[0061] (3) placing the transparent solution obtained in step (2) in a hydrothermal reactor for crystallization at a temperature of 160° C. for 3 h;

[0062] (4) centrifuging the milky white suspension obtained in step (3) at a speed of 6000-10000 rpm, washing with a mixed solution of ethanol: deionized water = 1:1, and drying at 80°C to obtain a white solid powder;

[0063] (5) The white powder obtained in step (4) is calcined once in an air atmosphere at a temperature of 600° C. for 4 h at a heating rate of 2° C. / min to obtain a white powder, namely aluminum oxide (Al 2 O 3 ).

[0064] Example 2 Preparation of alumina support (WO3 / Al2O3) by one-step synthesis method

[0065] (1) 0.088 g of ammonium metatungstate was dissolved in 50 mL of water to make it uniformly dispersed, and 0.5 g of alumina powder obtained in Example 1 was added. The mixture was stirred at 600 rpm for 2 h. The temperature of the rotary evaporation was 60° C. and the speed was 130 r / min.

[0066] (2) The powder obtained by rotary evaporation in step (1) was subjected to secondary calcination in an air atmosphere at a temperature of 600° C. for 4 hours at a heating rate of 2° C. / min. The resulting white powder was tungsten oxide-alumina carrier (WO3 / Al2O3).

[0067] Example 3 Construction of palladium-tungsten oxide dual active sites using oil bath method

[0068] (1) 0.2 g of the WO3 / Al2O3 solid powder prepared in Example 2 was dissolved in 45 mL of deionized water and stirred at 600 rpm for 30 min to make it uniformly dispersed; the pH was adjusted to 10 with 0.25 mol / L anhydrous sodium carbonate solution, and the stirring was continued to make it uniform to obtain a mixed solution.

[0069] (2) After heating the mixed solution obtained in step (1) to 100° C., 5 mL of a 0.0004 g / mL aqueous palladium nitrate solution was added dropwise, and stirring was continued at 600 rpm for 1 h to obtain a solution.

[0070] (3) After the solution obtained in step (2) cools to room temperature, the solution is centrifuged at 8000 rpm, washed with deionized water for 6 times, and vacuum dried at 60° C. to obtain a light yellow solid powder;

[0071] (4) The light yellow solid powder obtained in step (3) was calcined in a hydrogen-argon atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 10%) at a flow rate of 150 mL / min, a temperature of 200° C., and a time of 1 h to finally obtain a highly active bifunctional catalyst Pd / WO3 / Al2O3.

[0072] See also Figure 1 In (a), (b) and (c), the high-activity bifunctional catalytic material prepared in Example 3 of the present invention presents an obvious two-dimensional layered structure.

[0073] See also Figure 2 In (a), (b) and (c), from Figure 2 The results show that the high-activity bifunctional catalytic material tungsten oxide prepared in Example 3 of the present invention is clearly dispersed at the atomic level, and the palladium clusters are evenly distributed.

[0074] See also Figure 3The high-activity bifunctional catalytic material prepared in Example 3 of the present invention has good crystallinity and clear crystal phase.

[0075] Example 4

[0076] (1) Dissolve 3 mmol (1.13 g) aluminum nitrate nonahydrate and 6 mmol (0.36 g) urea in 70 mL of deionized water and stir at 500 rpm for 20 min to disperse them evenly;

[0077] (2) 10 mL of ethanol was added dropwise to the clear solution obtained in step (1), followed by addition of 0.25 g of dodecylamine, and the mixture was stirred at a rotation speed of 500 r / min for 60 min to achieve uniform dispersion;

[0078] (3) The transparent solution obtained in step (2) was carefully placed in a hydrothermal reactor and reacted at 160° C. for 3 h;

[0079] (4) centrifuging the milky white suspension obtained in step (3), washing it five times with a mixture of ethanol and deionized water (volume ratio 1:1), and drying it at 90° C. to obtain a white solid powder;

[0080] (5) The white powder obtained in step (4) was preliminarily calcined in a muffle furnace at a temperature of 550° C. for 4 h at a heating rate of 2° C. / min to obtain a powder;

[0081] (6) Dissolve 0.088 g of ammonium metatungstate in 50 mL of water, stir to make it evenly dispersed, then add 0.5 g of the powder obtained by preliminary calcination in step (5), and stir at 600 rpm for 4 h. After the reaction is completed, transfer to a rotary evaporator, set the water bath temperature to 60°C, and the speed to 130 r / min;

[0082] (7) calcining the powder obtained by rotary evaporation in step (6) in a muffle furnace at a temperature of 600° C. for 4 h with a heating rate of 2° C. / min;

[0083] (8) Accurately weigh 0.2 g of the powder obtained by the second calcination in step (7), dissolve it in 45 mL of water, and stir for 30 min to make it evenly dispersed. Then adjust the pH to 9.5 with 0.25 mol / L anhydrous sodium carbonate solution, and stir continuously until the mixture is evenly mixed;

[0084] (9) heating the solution in step (8) to 100° C., adding 5 mL of a 0.0006 g / mL aqueous palladium nitrate solution dropwise, and stirring continuously at 800 rpm for 1.5 h;

[0085] (10) After the reaction in step (9) is completed, the mixed solution is cooled to room temperature, centrifuged at a speed of 9000 r / min, washed with deionized water for 6 times, and then dried in a vacuum at 60° C. to obtain a light yellow solid powder;

[0086] (11) In a H2 / Ar atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere is 10%), the powder obtained in step (10) is calcined at a flow rate of 200 mL / min and a temperature of 200°C for 2 h to finally prepare a high-activity bifunctional catalyst Pd / WO3 / Al2O3 of palladium-atomic-dispersed tungsten oxide.

[0087] Example 5

[0088] 0.2 g of the WO3 / Al2O3 carrier obtained in Example 2 was accurately weighed into 45 ml of DI water and stirred at 700 r / min for 45 min to be uniformly dispersed.

[0089] The pH value of the mixed solution was adjusted to 10.5 with 0.25 mol / L anhydrous sodium carbonate solution, and stirring was continued until the mixture was uniform. When the mixed solution was heated to 100°C, 5 mL of 0.0006 g / mL of palladium nitrate aqueous solution was added dropwise, and stirring was continued for 1 hour at a rotation speed of 800 r / min. After the reaction was completed, the solution was cooled to room temperature, centrifuged at a speed of 10000 r / min, washed with deionized water 7 times, and then dried in a vacuum at 60°C. The obtained light yellow solid powder was calcined at 200°C for 1 hour in a hydrogen-argon atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 10%) at a flow rate of 100 mL / min to obtain a high-activity bifunctional catalyst Pd / WO3 / Al2O3 of palladium-atomic dispersed tungsten oxide.

[0090] Example 6

[0091] (1) Dissolve 6 mmol (2.26 g) of aluminum nitrate nonahydrate and 12 mmol (0.72 g) of urea in 71 ml of DI water and stir at 500 rpm for 30 min to make them evenly dispersed;

[0092] (2) 11 mL of ethanol was added dropwise to the clear solution obtained in step (1), followed by 0.50 g of dodecylamine, and the mixture was stirred at 500 r / min for 40 min to allow uniform dispersion;

[0093] (3) Pour the clear solution obtained in step (2) into a 100 mL hydrothermal reaction kettle and perform a hydrothermal reaction at 160° C. for 5 h;

[0094] (4) After the hydrothermal reaction is completed and the temperature is lowered to room temperature, the mixed solution obtained in step (3) is centrifuged and washed five times with a mixed solution of ethanol and deionized water (1:1.2), and dried at 100° C. to obtain a white powder;

[0095] (5) calcining the white powder obtained in step (4) for the first time in a muffle furnace at a temperature of 550° C., a calcination time of 6 h, and a heating rate of 5° C. / min;

[0096] (6) Dissolve 0.066 g of ammonium metatungstate in 50 mL of deionized water, stir thoroughly, and then stir at 800 rpm for 2 hours. After the reaction is completed, perform rotary evaporation at a water temperature of 60°C and a rotation speed of 125 r / min;

[0097] (7) The powder obtained in step (6) was calcined in a muffle furnace at 600° C. for 5 h with a heating rate of 2° C. / min to obtain a WO3 / Al2O3 carrier.

[0098] (8) Accurately weigh 0.2 g of the WO3 / Al2O3 carrier obtained in step (7), dissolve it in 45 mL of deionized water, and stir it for 40 min to make it evenly dispersed. Then, adjust the pH of the mixed solution to 10 with 0.25 mol / L anhydrous sodium carbonate solution, and continue stirring until it is completely uniform;

[0099] (9) The solution in step (8) was heated to 100° C., stirred continuously at 800 rpm, 5 mL of 0.0008 g / mL palladium nitrate aqueous solution was added dropwise, and stirring was continued for 1 h;

[0100] (10) After the reaction in step (9) is completed, the mixed solution is cooled to room temperature and then centrifuged at 8500 r / min, washed with deionized water for 6 times, and then dried in a vacuum drying oven at 60° C. to obtain a light yellow solid powder;

[0101] (11) The obtained light yellow solid powder was calcined at 200 °C for 1 h in a H2 / Ar atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 5%) at 200 mL / min to obtain a highly active bifunctional catalyst, which was denoted as Pd / WO3 / Al2O3.

[0102] Example 7

[0103] (1) Dissolve 4 mmol of aluminum nitrate nonahydrate and 8 mmol of urea in 65 ml of DI water and stir at 450 rpm for 30 min to make them evenly dispersed;

[0104] (2) 8 mL of ethanol was added dropwise to the clear solution obtained in step (1), followed by 0.35 g of dodecylamine, and the mixture was stirred at 500 r / min for 40 min to allow uniform dispersion;

[0105] (3) Pour the clear solution obtained in step (2) into a 100 mL hydrothermal reactor and perform a hydrothermal reaction at 155° C. for 4 h;

[0106] (4) After the hydrothermal reaction is completed and the temperature is lowered to room temperature, the mixed solution obtained in step (3) is centrifuged at 6000 rpm, washed five times with a mixed solution of ethanol and deionized water (1:1.4), and dried at 80° C. to obtain a white powder;

[0107] (5) calcining the white powder obtained in step (4) for the first time in a muffle furnace at a temperature of 600° C., a calcination time of 5 h, and a heating rate of 2° C. / min;

[0108] (6) Dissolve 0.033 g of ammonium metatungstate in 50 mL of deionized water, stir thoroughly, and then stir at 400 rpm for 6 hours. After the reaction is completed, perform rotary evaporation at a water temperature of 60°C and a rotation speed of 130 r / min;

[0109] (7) The powder obtained in step (6) was calcined in a muffle furnace at 600° C. for 4 h with a heating rate of 2° C. / min to obtain a WO3 / Al2O3 carrier.

[0110] (8) Accurately weigh 0.2 g of the WO3 / Al2O3 carrier obtained in step (7), dissolve it in 47 mL of deionized water, and stir it for 40 min to make it evenly dispersed. Then, adjust the pH of the mixed solution to 6 with 0.25 mol / L anhydrous sodium carbonate solution, and continue stirring until it is completely uniform;

[0111] (9) The solution in step (8) was heated to 100° C., stirred continuously at 600 rpm, 5 mL of a 0.0005 g / mL aqueous palladium chloride solution was added dropwise, and stirring was continued for 2 h;

[0112] (10) After the reaction in step (9) is completed, the mixed solution is cooled to room temperature and then centrifuged at 7000 r / min, washed with deionized water for 6 times, and then dried in a vacuum drying oven at 50° C. to obtain a light yellow solid powder;

[0113] (11) The obtained light yellow solid powder was calcined at 300 °C for 1 h in a H2 / Ar atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 5%) at 170 mL / min to obtain a highly active bifunctional catalyst, which was denoted as Pd / WO3 / Al2O3.

[0114] Example 8

[0115] (1) Dissolve 6 mmol of aluminum nitrate nonahydrate and 12 mmol of urea in 68 ml of DI water and stir at 600 rpm for 30 min to make them evenly dispersed;

[0116] (2) 12 mL of ethanol was added dropwise to the clear solution obtained in step (1), followed by 0.5 g of dodecylamine, and the mixture was stirred at 400 r / min for 60 min to allow uniform dispersion;

[0117] (3) Pour the clear solution obtained in step (2) into a 100 mL hydrothermal reaction kettle and perform a hydrothermal reaction at 170° C. for 3 h;

[0118] (4) After the hydrothermal reaction is completed and the temperature is lowered to room temperature, the mixed solution obtained in step (3) is centrifuged at 10,000 rpm, washed five times with a mixture of ethanol and deionized water (1:1), and dried at 120° C. to obtain a white powder;

[0119] (5) calcining the white powder obtained in step (4) for the first time in a muffle furnace at a temperature of 650° C., a calcination time of 4 h, and a heating rate of 3° C. / min;

[0120] (6) Dissolve 0.11 g of ammonium metatungstate in 50 mL of deionized water, stir thoroughly, and then stir at 800 rpm for 2 hours. After the reaction is completed, perform rotary evaporation at a water temperature of 70°C and a rotation speed of 140 r / min;

[0121] (7) The powder obtained in step (6) was calcined in a muffle furnace at 600° C. for 6 h with a heating rate of 5° C. / min to obtain a WO3 / Al2O3 carrier.

[0122] (8) Accurately weigh 0.2 g of the WO3 / Al2O3 carrier obtained in step (7), dissolve it in 50 mL of deionized water, and stir it for 40 min to make it evenly dispersed. Then, adjust the pH of the mixed solution to 11 with 0.25 mol / L anhydrous sodium carbonate solution, and continue stirring until it is completely uniform;

[0123] (9) The solution in step (8) was heated to 110° C., stirred continuously at 700 rpm, and 5 mL of a 0.00015 g / mL sodium tetrachloropalladate aqueous solution was added dropwise, and stirring was continued for 1 h;

[0124] (10) After the reaction in step (9) is completed, the mixed solution is cooled to room temperature and then centrifuged at 9000 r / min, washed with deionized water for 6 times, and then dried in a vacuum drying oven at 70° C. to obtain a light yellow solid powder;

[0125] (11) The light yellow solid powder was calcined at 250 °C for 1.5 h under a H2 / Ar atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 10%) at 150 mL / min to obtain a highly active bifunctional catalyst, which was denoted as Pd / WO3 / Al2O3.

[0126] Example 9

[0127] (1) Dissolve 3 mmoL aluminum nitrate nonahydrate and 6 mmoL urea in 75 ml DI water and stir at 400 rpm for 30 min to make them evenly dispersed;

[0128] (2) 10 mL of ethanol was added dropwise to the clear solution obtained in step (1), followed by 0.25 g of dodecylamine, and the mixture was stirred at 600 r / min for 30 min to allow uniform dispersion;

[0129] (3) Pour the clear solution obtained in step (2) into a 100 mL hydrothermal reaction kettle and perform a hydrothermal reaction at 150° C. for 5 h;

[0130] (4) After the hydrothermal reaction is completed and the temperature is lowered to room temperature, the mixed solution obtained in step (3) is centrifuged at 8000 rpm, washed 5 times with a mixed solution of ethanol and deionized water (1:1.5), and dried at 110° C. to obtain a white powder;

[0131] (5) calcining the white powder obtained in step (4) for the first time in a muffle furnace at a temperature of 550° C., a calcination time of 6 h, and a heating rate of 5° C. / min;

[0132] (6) Dissolve 0.00275 g of ammonium metatungstate in 50 mL of deionized water, stir thoroughly, and then stir at 600 rpm for 4 hours. After the reaction is completed, perform rotary evaporation at a water temperature of 50°C and a rotation speed of 120 r / min;

[0133] (7) The powder obtained in step (6) was calcined in a muffle furnace at 620° C. for 5 h with a heating rate of 4° C. / min to obtain a WO3 / Al2O3 carrier.

[0134] (8) Accurately weigh 0.2 g of the WO3 / Al2O3 carrier obtained in step (7), dissolve it in 45 mL of deionized water, and stir it for 40 min to make it uniformly dispersed. Then, adjust the pH of the mixed solution to 8 with 0.25 mol / L anhydrous sodium carbonate solution, and continue stirring until it is completely uniform;

[0135] (9) The solution in step (8) was heated to 90° C., stirred continuously at 650 rpm, and 5 mL of a 0.0008 g / mL aqueous palladium nitrate solution was added dropwise, and stirring was continued for 1.5 h;

[0136] (10) After the reaction in step (9) is completed, the mixed solution is cooled to room temperature and then centrifuged at 6000 r / min, washed with deionized water for 6 times, and then dried in a vacuum drying oven at 60° C. to obtain a light yellow solid powder;

[0137] (11) The obtained light yellow solid powder was calcined at 270°C for 1 h in a H2 / Ar atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 7%) at 120 mL / min to obtain a highly active bifunctional catalyst, which was denoted as Pd / WO3 / Al2O3.

[0138] Comparative Example 1

[0139] (1) 0.2 g of Al2O3 solid powder prepared in Example 1 was accurately weighed, placed in 45 ml of DI (deionized) water, and stirred at 600 rpm for 40 min to disperse uniformly; the pH value was adjusted to 10 with 0.25 mol / L anhydrous sodium carbonate solution, and then stirred continuously until the mixture was uniformly mixed.

[0140] (2) After heating the mixed solution obtained in step (1) to 100° C., 5 mL of a 0.0004 g / mL aqueous palladium nitrate solution was added dropwise, and stirring was continued at a rotation speed of 620 r / min for 1 hour.

[0141] (3) After the solution obtained in step (2) is cooled to room temperature, it is centrifuged at a rotation speed of 8000 r / min, washed with deionized water for 5 times, and then dried in a vacuum drying oven at 60° C. to obtain a light yellow solid powder;

[0142] (4) In a hydrogen-argon atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere is 10%), the powder obtained in step (3) is subjected to reduction calcination at a heating rate of 150 mL / min, 200°C, 1 h, and 2°C / min to obtain a pure palladium catalytic material Pd / Al2O3.

[0143] Comparative Example 2

[0144] 0.2g of the alumina carrier obtained in Example 1 was dispersed in 45mL of deionized water and stirred at 800rpm for 40min to make it uniformly dispersed. The pH was adjusted to 10.5 with 0.25mol / L of anhydrous sodium carbonate solution, and stirring was continued to make it uniform. The mixed solution was heated to 100°C, and 5mL of a 0.0006g / mL aqueous palladium nitrate solution was added dropwise, and stirring was continued at 800rpm for 1.5h. After the reaction was completed, the solution was cooled to room temperature, centrifuged at 10000rpm, washed with deionized water, and vacuum dried at 60°C to obtain a light yellow solid powder. The obtained powder was calcined in a hydrogen-argon atmosphere (the volume percentage of hydrogen in the hydrogen-argon atmosphere was 10%), with a flow rate of 100mL / min, a temperature of 200°C, and a time of 2h, and finally a pure palladium catalytic material Pd / Al2O3 was obtained.

[0145] Example 10 Activity test of catalytic degradation of methyl ethyl ketone by high-activity bifunctional catalytic material:

[0146] The catalytic reaction was carried out in a fixed bed. The catalyst obtained in Example 3 was tableted and sieved (40-60 mesh). 0.2 g of the sieved catalyst was accurately weighed. Methyl ethyl ketone was used as a probe gas. The concentration of the reactants was controlled at 600 ppm. The reaction space velocity was 45000 h -1 , the oxygen volume concentration was 21%, and the catalytic reaction activity of the catalyst was tested at 40-260°C (interval 20°C), and the reaction products were monitored and analyzed by gas chromatography online mass spectrometry.

[0147] See also Figure 4-Figure 5 ,from Figure 4-Figure 5 The analysis shows that the high-activity bifunctional catalytic material Pd / WO3 / Al2O3 prepared in Example 3 of the present invention and the Pd / Al2O3 catalytic material prepared in Comparative Example 1 are applied to the catalytic oxidation of methyl ethyl ketone. The activity of Pd / Al2O3 for methyl ethyl ketone shows a decreasing trend in the temperature range of 100-140°C and cannot achieve deep mineralization. The high-activity bifunctional catalytic material Pd / WO3 / Al2O3 for methyl ethyl ketone shows excellent low-temperature degradation efficiency at 40-260°C and a space velocity of 45000h / min. -1 Under the condition of oxygen volume concentration of 21%, continuous deep oxidation of methyl ethyl ketone can be achieved. 90% of methyl ethyl ketone can be deeply purified at 140°C, and the CO2 generation rate can reach 90% at 168°C.

[0148] Example 11 Cyclic stability test of high activity bifunctional catalytic material:

[0149] The catalyst obtained in Example 3 was tableted and sieved (40-60 mesh). 0.2 g of the sieved catalyst material was accurately weighed and placed in a fixed bed of an evaluation device. It was activated at 200°C for 1 h. Methyl ethyl ketone was used as a probe gas. The concentration of the reactants was controlled at 600 ppm. The reaction space velocity was 45000 h -1 , oxygen concentration is 21%. Record the reaction activity after each temperature stabilizes at 40-200℃, cool down to room temperature after completing a catalytic reaction process, and then heat up again. Repeat this process five times to continuously test the catalytic reaction activity of the catalyst under mixed component atmosphere conditions.

[0150] See also Figure 6 ,from Figure 6 The results show that the high-activity bifunctional catalytic material prepared in Example 3 of the present invention has better cycle performance in the low-temperature purification of methyl ethyl ketone than the Pd / Al2O3 catalytic material prepared in Comparative Example 1. In the test of five cycles of heating-cooling-reheating, the T 90 Always stable, with excellent reaction stability.

[0151] Example 12 Long-term stability test of high-activity bifunctional catalytic material:

[0152] The catalyst obtained in Example 3 was tableted and sieved (40-60 mesh). 0.2 g of the sieved catalyst material was accurately weighed and placed in a fixed bed of an evaluation device. It was activated at 200°C for 1 h, cooled to 140°C and maintained. Methyl ethyl ketone was used as a probe gas. The concentration of the reactants was controlled at 600 ppm and the reaction space velocity was 45000 h -1 , oxygen concentration is 21%. The catalytic reaction activity of the catalyst under mixed component atmosphere conditions was continuously tested.

[0153] See also Figure 7 It can be seen that the high-activity bifunctional catalytic material prepared in Example 3 of the present invention maintains extremely excellent activity at 140°C during the test period of 700 hours without showing any downward trend, and has extremely strong reaction stability.

[0154] The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. All changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.

[0155] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

Claims

1. A method for preparing a highly active bifunctional catalytic material, characterized in that: The following steps are involved: Aluminum nitrate nonahydrate and urea are dissolved in deionized water, ethanol and a surfactant are added, and then crystallization is performed, centrifugation, washing, drying, and then calcination is performed once to obtain a calcined powder; The primary calcined powder is added to the ammonium metatungstate solution, and after stirring and reacting completely, a solid is obtained by rotary evaporation, and the solid is subjected to secondary calcination to obtain the final powder; The final powder is added to water to obtain a tungsten oxide-alumina carrier suspension, and the palladium salt solution is added after adjusting the pH to 6-11, and the reaction is carried out at 90-110°C for 1-2h to obtain a light yellow solid; The light yellow solid was calcined three times to obtain a highly active bifunctional catalytic material.

2. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The molar ratio of aluminum nitrate nonahydrate to urea is 3-6:6-12 mmoL.

3. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The surfactant was dodecylamine.

4. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The ratio of aluminum nitrate nonahydrate to ethanol is 3-6 mmol: 8-12 mL; The usage ratio of aluminum nitrate nonahydrate to surfactant is 3-6mmol:0.25-0.5g.

5. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The crystallization temperature is 150-170°C and the time is 3-5h; The primary calcination temperature is 550-650°C for 4-6 hours; the temperature is increased to 550-650°C at a heating rate of 2-5°C / min.

6. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The mass ratio of the primary calcined powder to ammonium metatungstate is 0.5g:0.00275-0.11g; The secondary calcination temperature is 600-650°C, and the time is 4-6h; the temperature is increased to 600-650°C at a heating rate of 2-5°C / min.

7. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The final powder and palladium salt solution dosage ratio is 0.2 g: 5 mL, and the concentration of the palladium salt solution is 0.00015-0.0006 g / mL; The palladium salt is palladium nitrate, palladium chloride or sodium tetrachloropalladate.

8. The method for preparing a highly active bifunctional catalytic material according to claim 1, characterized in that: The temperature of the three calcinations is 200-300°C and the time is 1-1.5h; the three calcinations are carried out under a mixture of hydrogen and argon; The volume percentage of hydrogen in the mixture of hydrogen and argon is 5-10%; The flow rate of the mixture of hydrogen and argon is 100-200 mL / min.

9. A high-activity bifunctional catalytic material prepared according to the method according to any one of claims 1 to 8, characterized in that: The specific surface area of ​​the catalytic material is 159.0-170.9 m 2 / g, micropore volume is 0.067-0.071cm 3 / g.

10. Use of a high-activity bifunctional catalytic material prepared by the method according to any one of claims 1 to 8 in the purification of volatile oxygen-containing hydrocarbons.

Citation Information

Patent Citations

  • Supported catalyst for eliminating formaldehyde, preparation method and application thereof

    CN101559377A

  • Formaldehyde oxidation composite catalytic material and preparation method thereof

    CN109759080A

  • Application of multi-active component catalyst to preparation of 1,3-propylene glycol by glycerol hydrogenolysis

    CN110560057A

  • Pd-based catalyst as well as preparation method and application thereof

    CN114100607A