Bouquet-shaped amorphous Co-P-B alloy material and preparation and application thereof
By using bouquet-like amorphous Co-P-B alloy materials as catalysts in aqueous solvents, the problems of low efficiency and poor stability of Co-based amorphous alloy catalysts in aqueous solvents are solved, and high-efficiency catalytic selective hydrogenation of furfural is achieved. Furfuryl alcohol was taken, and the thermal stability and recycling rate of the catalyst were improved through plasma treatment.
Patent Information
- Application Number
- CN202310317135.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing Co-based amorphous alloy catalysts have low catalytic efficiency in aqueous solvents, poor thermal stability, low recycling rate, and insufficient oxidation resistance, resulting in performance inactivation in industrial applications.
The bouquet-shaped amorphous Co-P-B alloy material is used, and the nanoribbon structure is formed in the layered liquid crystal by cobalt salt and complexing agent coordination and surfactant mixing, combined with the double reducing agent of sodium borohydride and sodium hypophosphite. , plasma treated to improve surface area and thermal stability, and regenerated in a plasma reactor.
It achieves efficient catalytic selective hydrogenation of furfural to produce furfuryl alcohol under mild conditions, improves the selectivity and conversion rate of the catalyst, extends the service life of the catalyst, and reduces energy consumption and environmental pollution.
Smart Images

Figure CN118720126A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a Co-PB alloy material, in particular to a bouquet-shaped amorphous Co-PB alloy material, and also to a preparation method of the bouquet-shaped amorphous Co-PB alloy material and application of the bouquet-shaped amorphous Co-PB alloy material as a catalyst in the selective hydrogenation of furfural to prepare furfuryl alcohol, belonging to the technical field of industrial catalysis. Background Art
[0002] The development of low-cost, available and renewable lignocellulosic biomass using efficient and pollution-free technologies has been attracting worldwide attention to alleviate the energy crisis and climate change caused by fossil fuels. It is of utmost importance to design efficient catalytic processes to convert lignocellulosic biomass into biofuels and fine chemicals. Furfural is a biomass-derived chemical. The further catalytic selective hydrogenation of furfural as a raw material to produce furfuryl alcohol has important research background and application prospects, because furfuryl alcohol is widely used as an intermediate in the synthesis of furan-based resins, fibers, lubricants, pharmaceuticals and microbial C. However, in the reaction process of furfural selective hydrogenation to furfuryl alcohol, there are always side reactions. Competitive hydrogenation of furan rings gives tetrahydrofurfural, furfuryl alcohol and tetrahydrofurfural are further hydrogenated to tetrahydrofurfuryl alcohol. When the addition reactions on the C=O and C=C bonds compete, obtaining high yields of furfuryl alcohol from furfural obviously requires artificial control of product selectivity. In addition, organic matter is mostly used as solvent in the process of furfuryl alcohol production by hydrogenation of furfural, which not only pollutes the environment but also requires separation after production. The relevant industries continue to demand the use of water to replace organic solvents. However, it is necessary to develop new high-efficiency catalysts that can selectively hydrogenate in pure water media.
[0003] Previously, supported noble metal and noble metal-non-noble metal catalysts were used to hydrogenate furfural to furfuryl alcohol in organic solvents, but rarely reported in aqueous media. This is because the active components of these catalysts have excellent reactivity in adsorbing and activating H2 molecules, and a large amount of by-products are produced due to over-hydrogenation. Studies have shown that supported Co as a cheap catalyst shows activity for the hydrogenation of furfural to furfuryl alcohol in water, but requires a fairly high H2 pressure (2-4 MPa). Therefore, improving the catalytic activity of Co-based catalysts for the selective reduction of C=O bonds in furfural is a cost-effective and environmentally friendly process, but it remains a huge challenge.
[0004] Amorphous catalysts with unique short-range ordered and long-range disordered atomic arrangements have attracted increasing attention from academia and industry due to their unique chemical and structural properties, including widely adjustable composition, uniform structure and high concentration of coordinated unsaturated sites. A series of Co-based amorphous catalysts have been used to catalyze the selective hydrogenation of furfural to furfuryl alcohol, which show good catalytic efficiency and low environmental pollution. However, their application and development are limited by factors such as poor thermal stability and low surface area. In order to enhance its competitiveness in industry, people adopt the following strategies to promote its application: the widely studied strategy is to modify Co-B amorphous alloy nanoparticles with different metal additives (such as Fe, Ni, Mo, W and Ce) and non-metal additives (such as P). H. Li, et al., (Appl. Catal. A: Gen. 325 (2007) 34-40.) and P. Li, et al., (Mater. Chem. 2 (2014) 18420.) studied this, but they found that the granular catalyst is easily deactivated by agglomeration during catalytic hydrogenation due to its high surface energy. Another strategy is to load the granular amorphous alloy on a carrier with a high surface area. The most commonly used carriers are SiO2, γ-Al2O3 and carbon nanotubes; in recent years, people have made amorphous alloys into different shapes, such as mesoporous spheres, wires, nanotubes, etc., in order to improve the structural stability of amorphous alloy nanocatalysts and thus improve their reuse rate. However, the biggest problem with amorphous alloy catalysts is their poor oxidation resistance, which causes the catalyst to deactivate during recycling. For amorphous alloy catalysts, if a good strategy can be found to solve the regeneration problem, the application of amorphous alloy catalysts in industry will be improved. Summary of the invention
[0005] In view of the problems in the prior art such as poor thermal stability, low recycling rate, difficulty in regeneration and low catalytic efficiency in water solvents of Co-based amorphous alloy nanomaterials, the first object of the present invention is to provide a bouquet-shaped amorphous Co-PB alloy material, which has the characteristics of high structural stability, high specific surface area and high catalytic activity.
[0006] The second object of the present invention is to provide a method for preparing a bouquet-shaped amorphous Co-PB alloy material, which has the advantages of high efficiency, simple and convenient operation, and low energy consumption.
[0007] The third object of the present invention is to provide an application of a bouquet-shaped amorphous Co-PB alloy material, which is used as a catalyst in the selective hydrogenation of furfural to prepare furfuryl alcohol, and can obtain a higher conversion rate and selectivity under mild conditions.
[0008] In order to achieve the above technical objectives, the present invention provides a bouquet-shaped amorphous Co-PB alloy material having a micron-scale bouquet structure; the micron-scale bouquet structure is assembled from a number of amorphous Co-PB alloy nanoribbons.
[0009] The bouquet-shaped amorphous Co-PB alloy material of the present invention is in the shape of a bouquet of nanosheets, which is not easy to agglomerate or collapse compared with other morphologies such as nanoparticles, nanowires, and nanotubes, and has better structural stability. In terms of composition, compared with Co-P and Co-B binary amorphous alloy nanomaterials, part of the free electrons on B are first transferred to the Co element, and P can accept electrons from Co. Due to the mutual transfer of electrons between the three elements, a synergistic effect is generated, so that the Co-PB alloy material has higher thermal stability.
[0010] As a preferred solution, the amorphous Co-PB alloy nanobelt comprises the following components in molar percentage: Co 65-69%; P 20-25%; B 10-11%.
[0011] As a preferred solution, the Co-PB amorphous alloy nanobelt has a width of 80 to 300 nm, the overall length of the micron-scale bouquet structure is 2 to 6 μm, and the center angle is 45 to 160°. The Co-PB amorphous alloy nanomaterial of the present invention has a wide range of center angles, which can increase the exposure of the catalytic active sites of the material, thereby improving the catalytic activity of the material.
[0012] The present invention also provides a method for preparing a bouquet-shaped amorphous Co-PB alloy material, which comprises dissolving a ligand and a cobalt salt into water under the action of a surfactant to obtain a precursor solution; adding an alkaline solution containing sodium hypophosphite and sodium borohydride to the precursor solution for reaction to obtain a bouquet-shaped amorphous Co-PB alloy material I; or further subjecting the bouquet-shaped amorphous Co-PB alloy to plasma treatment to obtain a bouquet-shaped amorphous Co-PB alloy material II.
[0013] The key to the present invention is that a cobalt salt is firstly coordinated with a coordinating agent to obtain a stable cobalt salt complex, which is then mixed with a surfactant and water to prepare a lamellar liquid crystal. The lamellar liquid crystal is then used as a template to reduce the Co in the liquid crystal precursor using a double reducing agent of sodium borohydride and sodium hypophosphite. 2+Reduction is carried out, and the molar ratio of Co, P, and B in the nanosheets is controlled by controlling the amount of raw materials, so as to limit the growth into thin bouquet-shaped Co-PB nanobelts in the water layer of the lamellar liquid crystal. The bouquet-shaped Co-PB nanobelts will have more surface active sites due to the scale effect, but due to the large amount of surfactants in the lamellar liquid crystal, the surface active sites in the newly prepared bouquet-shaped amorphous Co-PB alloy material will be covered in large quantities, resulting in an insufficient specific surface area and uneven surface active sites. The present invention combines the prepared bouquet-shaped amorphous Co-PB alloy material with plasma to treat the surface area of the bouquet-shaped amorphous Co-PB alloy material I, thereby increasing the surface area of the bouquet-shaped amorphous Co-PB alloy material I from 70 to 74 m 2 / g increased to 90~110m 2 / g, the specific surface area of the material is significantly improved and the surface active sites are more uniform, the adsorption capacity of H2 is enhanced, and the surface state of the material is also changed. In addition, plasma has a certain reduction effect on the bouquet-shaped amorphous Co-PB alloy material, changing the valence state of the metal active components, and the surface can produce more Co 0 , thereby improving the catalytic efficiency and selectivity of the selective hydrogenation of furfural to produce furfuryl alcohol.
[0014] As a preferred solution, the mass ratio of the surfactant to the complexing agent is 6-8:0.5-1.2, and the concentration of the cobalt salt is 0.1-1 mol / L.
[0015] As a preferred solution, the cobalt salt includes cobalt chloride or a hydrate of cobalt chloride, more preferably cobalt chloride hexahydrate. The surfactant is Tween, more preferably Tween 60.
[0016] As a preferred embodiment, the complexing agent includes D-(+) camphorsulfonic acid.
[0017] As a preferred solution, the molar ratio of Co:P:B in the cobalt salt, sodium hypophosphite and sodium borohydride is controlled to be 1:(1-4):2. The molar ratio of P to B in the present invention is crucial, and its dosage directly affects the microscopic morphology of the prepared Co-PB amorphous alloy nanobelts. As the molar ratio of P to B increases, the central angle of the bouquet of the prepared Co-PB amorphous alloy nanobelts will decrease. In the present invention, the content of P comes from sodium hypophosphite, and the content of B comes from sodium borohydride. Sodium hypophosphite and sodium borohydride are also reducing agents. At room temperature, sodium hypophosphite will not react with cobalt ions. Only under the initiation of sodium borohydride will sodium hypophosphite participate in the reduction together. If the proportion of sodium borohydride is too low, that is, the molar ratio of P to B is too high, the content of the obtained product is relatively small, and the prepared Co-PB amorphous alloy nanomaterials are mostly granular; while the proportion of sodium borohydride is too high, that is, the molar ratio of P to B is too low, the prepared Co-PB amorphous alloy nanomaterials will also produce too many particles, and the proportion of the generated nanoribbon products is very small.
[0018] As a preferred solution, the alkaline solution is pumped in at a speed of 0.05 to 0.10 mL / min. When the alkaline solution is pumped in at a speed that is too fast, the morphology of the prepared material cannot be effectively controlled.
[0019] As a preferred solution, the power of the plasma generator during the plasma treatment process is 150-200W, and the time is 100-500s. The bouquet-shaped amorphous Co-PB alloy material can be treated by a plasma generator to significantly increase the specific surface area of the material and provide more active sites; on the other hand, it can reduce the catalyst surface and produce more Co on the surface. 0 , plasma treatment can increase the number of material cycles; especially when the bouquet-shaped amorphous Co-PB alloy material is inactivated, it can be regenerated by the plasma generator to extend the material's service life and achieve resource reuse. If the power of the plasma generator is too small and the time is too short, the plasma generated will not have a strong effect on the modification of the material surface state; if the power of the plasma generator is too large and the time is too long, the plasma generated will easily damage the material morphology.
[0020] The present invention provides a method for preparing a bouquet-shaped amorphous Co-PB alloy material, which specifically comprises the following steps:
[0021] Step 1: Preparation of precursor
[0022] 6-8 g of Tween 60, 0.5-1.2 g of D-(+) camphorsulfonic acid and a cobalt salt with a concentration of 0.1-1 mol / L are added to water and mixed. The mixture is stirred in a water bath at 60-70° C. until a transparent solution is obtained, and then cooled to 20-25° C. in a water bath to obtain a precursor.
[0023] Step 2: Preparation of bouquet-shaped amorphous Co-PB alloy material I
[0024] In an inert atmosphere, at 20-25°C, an alkaline solution of sodium hypophosphite and sodium borohydride was continuously pumped into the precursor (the pumping speed was controlled to be 0.05-0.10 mL / min), stirred and fully reacted, washed with distilled water and centrifuged, repeated 3-4 times, then washed with anhydrous ethanol and centrifuged, repeated 3-4 times, and then dried in a vacuum drying oven at 28-32°C for 12-24 hours to obtain a bouquet-shaped amorphous Co-PB alloy material I. The molar ratio of (Co:P:B) in the reactants was 1:(1-4):2.
[0025] Step 3: Preparation of bouquet-shaped amorphous Co-PB alloy material II
[0026] The prepared bouquet-shaped amorphous Co-PB alloy material is placed in a quartz boat and placed in a plasma reactor. High-purity nitrogen is delivered to the plasma reactor through a gas distribution system, and a glow discharge is generated in the reactor through a plasma system. The power of the plasma generator is adjusted to 150-250W, and the time is set to 100-500s.
[0027] The present invention also provides an application of a bouquet-shaped amorphous Co-PB alloy material, which is used as a catalyst in the reaction of selective hydrogenation of furfural to prepare furfuryl alcohol, and a higher conversion rate and selectivity can be obtained under milder reaction conditions.
[0028] As a preferred solution, the performance evaluation of the catalytic furfural selective hydrogenation to produce furfuryl alcohol is briefly described as follows:
[0029] Step 1: Place 0.5 g of catalyst, 5 mL of furfural and 160 mL of distilled water into a 200 mL reactor;
[0030] Step 2: After sufficient stirring, the reactor is purged with N2 and H2 three times each to expel air. During the entire catalytic reaction process, the pressure of hydrogen is always maintained at a fixed value, the pressure range is 0.2-3.0 MPa, and the reaction temperature is set at a fixed temperature, the reaction temperature range is 50-100°C;
[0031] Step 3: The solution is taken out from the reactor regularly and analyzed by gas chromatograph.
[0032] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0033] 1) The present invention uses liquid crystal as a precursor, and adopts sodium borohydride and sodium hypophosphite as double reducing agents to reduce Co in the liquid crystal precursor. 2+ Reduction is performed to form a bouquet-shaped Co-PB ternary amorphous alloy nanomaterial formed by nanobelts. Compared with other synthesis methods such as electrodeposition and chemical plating, the reaction can be carried out at room temperature, without the need for electricity or heating, which has the advantage of saving energy; in terms of morphology and structure, the bouquet-shaped nanobelts are not easy to agglomerate or collapse compared to other morphologies such as nanoparticles, nanowires, and nanotubes, and have better structural stability; in terms of composition, compared to Co-P and Co-B binary amorphous alloy nanomaterials, the mutual synergy of P and B has higher thermal stability.
[0034] 2) The bouquet-shaped amorphous Co-PB alloy material prepared by the present invention can increase the specific surface area from 70 to 74 m 2 / g increased to 90~110m 2 / g, which is higher than the specific surface area of other amorphous alloy nanomaterials.
[0035] 3) The bouquet-shaped amorphous Co-PB alloy material prepared in the present invention is used as a catalyst to evaluate the catalytic performance of the selective hydrogenation of furfural to produce furfuryl alcohol in an aqueous phase. Compared with other Co-based catalysts, the solvent for the catalytic reaction can be environmentally friendly deionized water, the reaction temperature is 80°C, the H2 pressure is 1.2 MPa, the reaction conditions are milder, and higher conversion rates and selectivities can be obtained under mild reaction conditions.
[0036] 4) When preparing the bouquet-shaped amorphous Co-PB alloy material, the present invention uses a lamellar liquid crystal as a template. The lamellar liquid crystal is composed of a surfactant, which is restricted to grow into a thin nanosheet in the water layer of the lamellar liquid crystal. The catalyst has more surface active sites due to the scale effect, but the surface active sites of the newly prepared bouquet-shaped Co-PB amorphous alloy nanosheet catalyst are largely covered by the surfactant, resulting in an insufficient specific surface area and uneven surface active sites. After the newly prepared catalyst is treated with low-temperature plasma, the specific surface area of the catalyst is increased, the surface active sites are more uniform, and the adsorption capacity for H2 is enhanced; the surface state of the catalyst is also changed, and the plasma has a certain reduction effect on the catalyst, and the surface can produce more Co 0 These advantages improve the catalytic efficiency and selectivity of furfural selective hydrogenation to furfuryl alcohol. Compared with other methods, plasma is a fast, simple and convenient method for modifying amorphous alloy catalysts with low energy consumption.
[0037] 5) Amorphous alloy nanocatalysts are easily oxidized and deactivated during operation. The present invention studies the regeneration effect of plasma surface treatment technology on bouquet-shaped amorphous Co-PB alloy materials. It is found that after several cycles of application experiments, the catalyst can be treated with plasma for a certain period of time again to restore its activity, thereby achieving the purpose of extending the catalyst life. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for use in the embodiments or comparative examples. The following drawings only include some embodiments and comparative examples involved in the process of explaining the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0039] Figure 1 This is an electron microscope photograph of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 1 of the present invention.
[0040] Figure 2 This is an electron microscope photograph of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2 of the present invention.
[0041] Figure 3 This is an electron microscope photograph of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 3 of the present invention.
[0042] Figure 4 3 is the XRD spectrum of the bouquet-shaped amorphous Co-PB alloy material prepared in Examples 2, 4, 5 and 6 of the present invention.
[0043] Figure 5 An electron microscope photograph of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 5 of the present invention.
[0044] Figure 6 A graph showing the relationship between the performance of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2 of the present invention for selective hydrogenation of furfural catalyzed in water and the reaction temperature.
[0045] Figure 7 A graph showing the relationship between the performance of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2 of the present invention for selective hydrogenation of furfural in aqueous phase catalysis and the reaction pressure.
[0046] Figure 8 Performance diagram of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2 of the present invention for catalytic selective hydrogenation of furfural in different solvents.
[0047] Fig. 9A graph showing the relationship between the performance of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2 of the present invention in catalyzing the selective hydrogenation of furfural in water phase and the reaction time.
[0048] Fig.10 A graph showing the relationship between the performance of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 4 of the present invention for selective hydrogenation of furfural in aqueous phase catalysis and the reaction time.
[0049] Fig.11 A graph showing the relationship between the performance of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 5 of the present invention for selective hydrogenation of furfural catalyzed in water and the reaction time.
[0050] Fig.12 A graph showing the relationship between the performance of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 6 of the present invention for selective hydrogenation of furfural in aqueous phase catalysis and the reaction time.
[0051] Fig.13 A graph showing the performance of selective hydrogenation of furfural catalyzed by bouquet-shaped amorphous Co-PB alloy material II in aqueous phase as a function of the number of cycles in Application Example 8 of the present invention.
[0052] Fig.14 A graph showing the performance of selective hydrogenation of furfural catalyzed by bouquet-shaped amorphous Co-PB alloy material II in aqueous phase as a function of the number of cycles in Application Example 9 of the present invention.
[0053] Fig.15 Application Example 10 of the present invention is a graph showing the performance of selective hydrogenation of furfural catalyzed by bouquet-shaped amorphous Co-PB alloy material II in aqueous phase as a function of the number of cycles.
[0054] Fig.16 TEM image (low magnification) of bouquet-shaped amorphous Co-PB alloy material II after selective hydrogenation of furfural catalyzed by water phase in Application Example 10 of the present invention.
[0055] Fig.17 TEM image (high magnification) of bouquet-shaped amorphous Co-PB alloy material II after selective hydrogenation of furfural catalyzed by water phase in Application Example 10 of the present invention. DETAILED DESCRIPTION
[0056] The present invention will be described in detail with the following examples, but these examples are only for illustrating the present invention and the present invention is not limited thereto.
[0057] The product prepared by the present invention is subjected to structural analysis by the following means: a TECNAI F114 transmission electron microscope is used to perform morphological analysis of the product at an accelerating voltage of 200 kV; a HITACHI S4800 scanning electron microscope is used to perform morphological analysis of the product after heat treatment at an accelerating voltage of 5.0 kV; a Bruker D8 advance X-ray polycrystalline diffractometer is used to perform structural analysis of the product; an ASAP 2020 physical / chemical adsorption instrument is used to perform specific surface area and porosity analysis of the product; and an AutoChem TP-5080 automatic adsorption instrument is used to perform H2 programmed temperature desorption analysis.
[0058] Example 1
[0059] a) Weigh 1.16 g of D-(+) camphorsulfonic acid, dissolve in 9 mL of deionized water, add 6.6 g of Tween 60, stir evenly in a 65°C water bath, then add 1.19 g of cobalt chloride hexahydrate, stir to form a transparent solution, let stand in a 65°C water bath for 5 minutes, cool the solution to 25°C, set the cooling time to 2.5 hours, and continue to stand in a 25°C water bath for 2 hours.
[0060] b) A mixed solution of sodium borohydride, sodium hypophosphite and sodium hydroxide was freshly prepared, 0.38 g of sodium borohydride and 0.53 g of sodium hypophosphite monohydrate were dissolved in 5 mL of 0.1 mol / L sodium hydroxide solution (the molar ratio of Co:P:B was controlled to be 1:1:2), and the mixture was added to the solution obtained in step a) at a flow rate of 0.05 mL / min using a constant flow pump at 25° C., and the reaction was completed by stirring under nitrogen protection.
[0061] c) The product obtained in step b) was washed three times with deionized water and anhydrous ethanol respectively, and centrifuged to obtain a black substance, which was dried in a vacuum drying oven for 24 hours at a drying temperature of 30° C. After drying, it was stored in a nitrogen atmosphere for later use.
[0062] Transmission electron microscopy was used to characterize its morphology. Figure 1 The width of the bouquet-shaped amorphous Co-PB alloy material I is 80-300 nm, the overall length of the bouquet is 2-6 μm, and the central angle of the bouquet is about 150°. The specific surface area is shown in Table 1. The specific surface area of the bouquet-shaped amorphous Co-PB alloy material I prepared in this embodiment is 72.1 m 2 / g. Its composition is Co 68.9 P 20.5 B 10.6 .
[0063] Example 2
[0064] The difference between this embodiment and embodiment 1 is that the mixed solution of sodium borohydride, sodium hypophosphite and sodium hydroxide prepared in step b) is prepared by dissolving 0.38 g of sodium borohydride and 1.06 g of sodium hypophosphite monohydrate in 5 mL of 0.1 mol / L sodium hydroxide solution, and the molar ratio of Co:P:B is controlled to be 1:2:2.
[0065] The rest of the contents are the same as those described in Example 1.
[0066] Transmission electron microscopy was used to characterize its morphology. Figure 2 The width of the bouquet-shaped amorphous Co-PB alloy material I is 80-300 nm, the overall length of the bouquet is 2-6 μm, and the central angle of the bouquet is about 90°. The specific surface area is shown in Table 1. The specific surface area of the bouquet-shaped amorphous Co-PB alloy material I prepared in this embodiment is 73.9 m 2 / g. Its composition is Co 66.0 P 23.5 B 10.5 .
[0067] Example 3
[0068] The difference between this embodiment and embodiment 1 is that the mixed solution of sodium borohydride, sodium hypophosphite and sodium hydroxide prepared in step b) is prepared by dissolving 0.38 g of sodium borohydride and 2.12 g of sodium hypophosphite monohydrate in 5 mL of 0.1 mol / L sodium hydroxide solution, and the molar ratio of Co:P:B is controlled to be 1:4:2.
[0069] The rest of the contents are the same as those described in Example 1.
[0070] Transmission electron microscopy was used to characterize its morphology. Figure 3 The width of the bouquet-shaped amorphous Co-PB alloy material I is 80-300 nm, the overall length of the bouquet is 2-6 μm, and the center angle of the bouquet is about 50°. The specific surface area is shown in Table 1. The specific surface area of the bouquet-shaped amorphous Co-PB alloy material I prepared in this embodiment is 70.7 m 2 / g. Its composition is Co 65.4 P 24.3 B 10.3 .
[0071] Example 4
[0072] The bouquet-shaped amorphous Co-PB alloy material I obtained in Example 2 was treated with low-temperature plasma. The low-temperature plasma treatment process is as follows: the prepared bouquet-shaped amorphous Co-PB alloy material is placed in a quartz boat and placed in a plasma reactor. High-purity N2 is delivered to the plasma reactor through a gas distribution system, and a glow discharge is generated in the reactor through a plasma system. The power of the plasma generator is adjusted to 200W, and the time is set to 150s.
[0073] The crystal structure of the samples was determined by XRD. Figure 4 As shown in Table 1, the specific surface area of the bouquet-shaped amorphous Co-PB alloy material II prepared in this embodiment is 98.9 m 2 / g.
[0074] Example 5
[0075] The difference between this embodiment and embodiment 4 is that the plasma treatment time is set to 300 s.
[0076] The rest of the contents are the same as those described in Example 4.
[0077] The crystal structure of the samples was determined by XRD. Figure 4 As shown in Table 1, the specific surface area of the bouquet-shaped amorphous Co-PB alloy material II prepared in this embodiment is 108.4 m 2 / g. Transmission electron microscopy was used to characterize its morphology, such as Figure 5 The plasma treatment did not destroy the morphology of the sample, which was still in the form of a thin ribbon with a width of 90 to 200 nm.
[0078] Example 6
[0079] The difference between this embodiment and embodiment 4 is that the plasma treatment time is set to 450 s.
[0080] The rest of the contents are the same as those described in Example 4.
[0081] The crystal structure of the samples was determined by XRD. Figure 4 As shown in Table 1, the specific surface area of the bouquet-shaped amorphous Co-PB alloy material II prepared in this embodiment is 109.1 m 2 / g.
[0082] Application Example 1
[0083] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction process, the hydrogen pressure was always maintained at 1.2 MPa, the reaction temperature was set at 50, 60, 70, 80, 90 and 100 ° C, and the reaction time was 2 h. After the reaction, the solution was taken out from the reactor and analyzed using a GC-2014 gas chromatograph.
[0084] The experimental results are as follows Figure 6 As shown: There are two products of furfural selective hydrogenation catalyzed by Co-PB amorphous alloy nanobelts in water phase, namely furfural alcohol and tetrahydrofurfuryl alcohol. As the temperature increases from 50°C to 100°C, the furfural conversion rate increases from 28.5% to 100%. From 50°C to 80°C, the furfural alcohol selectivity decreases slightly from 96.2% to 93.3%; when it exceeds 80°C, the furfural alcohol selectivity drops rapidly to 57.9%, while the tetrahydrofurfuryl alcohol selectivity increases rapidly from 6.8% to 42.1%.
[0085] Application Example 2
[0086] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction process, the reaction temperature was always maintained at 80°C, the H2 pressure was set to 0.2, 0.4, 0.8, 1.2, 1.6, 2.0 and 3.0 MPa, respectively, and the reaction time was 2 h. After the reaction, the solution was taken out of the reactor and analyzed using a GC-2014 gas chromatograph.
[0087] The experimental results are as follows Figure 7 As shown: There are two products of furfural selective hydrogenation catalyzed by Co-PB amorphous alloy nanobelts in water phase, namely furfural alcohol and tetrahydrofurfuryl alcohol. The relationship between the catalytic performance of Co-PB amorphous alloy nanobelts and H2 pressure tested at 80°C. As the H2 pressure increased from 0.2MPa to 1.2MPa, the furfural conversion increased from 16.1% to 76.0%. After that, with the further increase of H2 pressure, the furfural conversion increased slowly. Within the 1.2MPa H2 pressure range, the furfural alcohol selectivity increased slightly from 92.4% to 93.3%. At 3.0MPa H2 pressure, the furfural alcohol selectivity decreased significantly to 69.7%, and the tetrahydrofurfuryl alcohol selectivity increased to 30.3%.
[0088] Application Example 3
[0089] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2, 5 mL of furfural and 160 mL of solvent (1-propanol, ethanol, methanol and water, respectively) were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction process, the reaction temperature was always maintained at 80°C, the H2 pressure was always maintained at 1.2 MPa, and the reaction time was 2 h. After the reaction was completed, the solution was taken out from the reactor and analyzed using a GC-2014 gas chromatograph.
[0090] The experimental results are as follows Figure 8 As shown: Bouquet-shaped amorphous Co-PB alloy material I catalyzes the selective hydrogenation of furfural in 1-propanol, ethanol, methanol and water. There are two catalytic products, furfuryl alcohol and tetrahydrofurfuryl alcohol. The solvent has an effect on the furfural conversion rate and product selectivity. Among the four solvents, the furfural conversion rate in H2O is the highest, but the furfuryl alcohol selectivity is not the best, slightly lower than methanol.
[0091] Application Example 4
[0092] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material I prepared in Example 2, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction process, the hydrogen pressure was always maintained at 1.2 MPa, and the reaction temperature was set at 80°C. The solution was taken every 20 minutes and analyzed using a GC-2014 gas chromatograph.
[0093] The experimental results are as follows Fig. 9 As shown: Co-PB amorphous alloy nanobelts catalyze the selective hydrogenation of furfural in water phase to produce two products, furfuryl alcohol and tetrahydrofurfuryl alcohol. It can be seen that with the extension of time, the furfural conversion rate increases and the furfuryl alcohol selectivity decreases. It takes 220 minutes for furfural to be fully converted, and the selectivity of furfuryl alcohol is 87% when it is fully converted.
[0094] Application Example 5
[0095] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 4, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction, the hydrogen pressure was always maintained at 1.2 MPa, and the reaction temperature was set at 80°C. The solution was taken every 20 minutes and analyzed using a GC-2014 gas chromatograph.
[0096] The experimental results are as follows Fig.10As shown: The bouquet-shaped amorphous Co-PB alloy material II catalyzes the selective hydrogenation of furfural in the water phase to produce two products, namely furfuryl alcohol and tetrahydrofurfuryl alcohol. It can be seen that with the extension of time, the furfural conversion rate increases and the furfuryl alcohol selectivity decreases. It takes 140 minutes for furfural to be fully converted. When it is fully converted, the selectivity of furfuryl alcohol is 94%.
[0097] Application Example 6
[0098] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 5, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction process, the hydrogen pressure was always maintained at 1.2 MPa, and the reaction temperature was set at 80°C. The solution was taken every 20 minutes and analyzed using a GC-2014 gas chromatograph.
[0099] The experimental results are as follows Fig.11 As shown: The bouquet-shaped amorphous Co-PB alloy material II catalyzes the selective hydrogenation of furfural in the water phase to produce two products, namely furfuryl alcohol and tetrahydrofurfuryl alcohol. It can be seen that with the extension of time, the furfural conversion rate increases and the furfuryl alcohol selectivity decreases. It takes 100 minutes for furfural to be fully converted. When it is fully converted, the selectivity of furfuryl alcohol is 96.9%.
[0100] Application Example 7
[0101] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 6, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction process, the hydrogen pressure was always maintained at 1.2 MPa, and the reaction temperature was set at 80°C. The solution was taken every 20 minutes and analyzed using a GC-2014 gas chromatograph.
[0102] The experimental results are as follows Fig.12 As shown: There are two products of furfural selective hydrogenation catalyzed by bouquet-shaped amorphous Co-PB alloy material II in water phase, namely furfuryl alcohol and tetrahydrofurfuryl alcohol. The time for complete conversion of furfural and the selectivity of furfuryl alcohol are 80 minutes and 95.8%, respectively. When the reaction time is extended to 100 minutes, the selectivity of furfuryl alcohol is 94.2%.
[0103] Application Example 8
[0104] 0.5 g of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 5, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; after sufficient stirring, the reactor was purged with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction, the hydrogen pressure was always maintained at 1.2 MPa, the reaction temperature was set at 80 ° C, and the reaction time was 80 min. The above experiment was repeated 6 times, and the solution was taken out after each cycle experiment and analyzed with a GC-2014 gas chromatograph.
[0105] The experimental results are as follows Fig.13 As shown: In the first four cycles, the furfural conversion did not change significantly, but the furfural alcohol selectivity decreased slightly. However, in the 5th and 6th cycles, the furfural conversion and furfural alcohol selectivity decreased significantly.
[0106] Application Example 9
[0107] Take 0.5g of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 5, 5mL of furfural and 160mL of distilled water and place them in a 200mL reactor; after sufficient stirring, purge the reactor with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction, the pressure of hydrogen was always maintained at 1.2MPa, the reaction temperature was set at 80°C, and the reaction time was 80min. Repeat the above experiment 4 times. After centrifugation, washing and drying, the catalyst was treated with nitrogen atmosphere plasma at a power of 200W. After 150s, continue to repeat the above catalytic experiment 4 times. Take out the solution after each cycle experiment and analyze it with a GC-2014 gas chromatograph.
[0108] The experimental results are as follows Fig.14 As shown: In the four cycles, the furfural conversion rate and the furfuryl alcohol selectivity are very high, indicating that the catalytic performance of the sample can be restored after plasma treatment, and plasma can regenerate this type of catalyst.
[0109] Application Example 10
[0110] Take 0.5g of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 5, 5mL of furfural and 160mL of distilled water and place them in a 200mL reactor; after sufficient stirring, purge the reactor with N2 and H2 three times each to exhaust the air. During the entire catalytic reaction, the pressure of hydrogen was always maintained at 1.2MPa, the reaction temperature was set at 80°C, and the reaction time was 80min. Repeat the above experiment 4 times. After centrifugation, washing and drying of the catalyst, it was treated with nitrogen atmosphere plasma at a power of 200W. After 150s, the above catalytic experiment was repeated 4 times. Four cycles of application experiments were used as a cycle. After each cycle was completed, the catalyst was centrifuged, washed, dried and treated with nitrogen atmosphere plasma at a power of 200W. After 150s, the cycle application experiment was carried out again. After the 8th plasma treatment, the cycle application experiment was carried out again. After each cycle experiment, the solution was taken out and analyzed with a GC-2014 gas chromatograph.
[0111] The catalytic test results are as follows Fig.15 As shown: The activity of the bouquet-shaped amorphous Co-PB alloy material II in catalyzing the selective hydrogenation of furfural to produce furfuryl alcohol is greatly reduced. Through TEM testing, such as Fig.16 (low magnification) and 17 (high magnification), it was found that the bouquet-like morphology of the catalyst was destroyed after this cycle, but the nanobelt morphology was still clearly visible, and the catalyst was still an amorphous structure ( Fig.16 ), but some nanoribbons have holes ( Fig.17 ).
[0112] Comparative Example 1
[0113] The difference between this comparative example and Example 2 is that the mixed solution of sodium borohydride, sodium hypophosphite and sodium hydroxide prepared in step b) is prepared by dissolving 0.19 g of sodium borohydride and 1.06 g of sodium hypophosphite monohydrate in 5 mL of 0.1 mol / L sodium hydroxide solution, and the molar ratio of Co:P:B is controlled to be 1:1:1.
[0114] The rest of the contents are the same as those described in Example 2.
[0115] After washing and centrifugation, the mass of the product obtained is less than that of Example 2. The morphology thereof was characterized by transmission electron microscopy, and most of the products were in the form of nanoparticles, with only a small amount of ribbon-like products being generated. The specific surface area is shown in Table 1. The specific surface area of the granular amorphous Co-PB alloy material I prepared in this comparative example is 31.9 m 2 / g. Its composition is Co 63.3 P 1.9 B 34.8 .
[0116] 0.5 g of sample, 5 mL of furfural and 160 mL of distilled water were placed in a 200 mL reactor; the hydrogen pressure was always maintained at 1.2 MPa, the reaction temperature was set at 80° C., and a selective hydrogenation reaction of furfural was carried out in the aqueous phase.
[0117] The experimental results show that the granular amorphous Co-PB alloy material catalyzes the selective hydrogenation of furfural in water phase to produce two products, namely furfuryl alcohol and tetrahydrofurfuryl alcohol. After 220 minutes of catalytic reaction, the furfural conversion rate is only 57.3%, and the selectivity of furfuryl alcohol is 79.1%.
[0118] Comparative Example 2
[0119] The difference between this comparative example and comparative example 1 is that the mixed solution of sodium borohydride, sodium hypophosphite and sodium hydroxide prepared in step b) is prepared by dissolving 0.57 g of sodium borohydride and 2.12 g of sodium hypophosphite monohydrate in 5 mL of 0.1 mol / L sodium hydroxide solution, and the molar ratio of Co:P:B is controlled to be 1:4:3.
[0120] The rest of the contents are the same as those described in Comparative Example 1.
[0121] The morphology was characterized by transmission electron microscopy. Most of the products were ribbon-shaped, but there were also many nanoparticles. The ribbons did not form a bouquet. The specific surface area is shown in Table 1. The specific surface area of the amorphous Co-PB alloy material I prepared in this comparative example is 58.2 m 2 / g. Its composition is Co 66.8 P 23.1 B 10.1 The experimental results of catalytic furfural selective hydrogenation showed that there were two products of furfural selective hydrogenation catalyzed by amorphous Co-PB alloy in water phase, namely furfural alcohol and tetrahydrofurfuryl alcohol. After 220 minutes of catalytic reaction, the furfural conversion rate was 79.6% and the furfural alcohol selectivity was 82.3%.
[0122] Comparative Example 3
[0123] The difference between this comparative example and Example 4 is that the bouquet-shaped amorphous Co-PB alloy material I obtained in Example 2 is treated with low-temperature plasma. The power of the plasma generator is adjusted to 100 W, and the time is set to 90 s.
[0124] The rest of the contents are the same as those described in Example 4.
[0125] The specific surface area is shown in Table 1. The specific surface area of the bouquet-shaped amorphous Co-PB alloy material II prepared in this comparative example is 73.2 m 2 / g. Compared with the bouquet-shaped amorphous Co-PB alloy material I described in Example 2, the specific surface area is 72.1m 2 / g, the specific surface area did not change much before and after treatment. The experimental results of catalytic furfural selective hydrogenation showed that there were two products of furfural selective hydrogenation catalyzed by amorphous Co-PB alloy in water phase, namely furfuryl alcohol and tetrahydrofurfuryl alcohol. It also took 220 minutes for furfural to be completely converted, and the selectivity of furfuryl alcohol was 83.1%, and the catalytic performance was not significantly improved.
[0126] Comparative Example 4
[0127] The difference between this comparative example and comparative example 3 is that the bouquet-shaped amorphous Co-PB alloy material I obtained in example 2 is treated with low-temperature plasma. The power of the plasma generator is adjusted to 250 W, and the time is set to 600 s. The rest of the contents are the same as those described in comparative example 3.
[0128] The sample tested by XRD is an amorphous structure. The specific surface area is shown in Table 1. The specific surface area of the bouquet-shaped amorphous Co-PB alloy material II prepared in this embodiment is 101.4 m 2 / g. Compared with the specific surface area of the bouquet-shaped amorphous Co-PB alloy material II prepared in Example 6, which is 109.1m 2 / g, the specific surface area is slightly decreased. The experimental results of catalytic furfural selective hydrogenation show that the amorphous Co-PB alloy material described in this comparative example catalyzes the selective hydrogenation of furfural in the water phase to produce two products, namely furfuryl alcohol and tetrahydrofurfuryl alcohol. It takes 100 minutes for furfural to be completely converted, and the selectivity of furfuryl alcohol is 91.8%. The catalytic performance is relative to that of application example 6, and the selectivity of furfuryl alcohol is decreased, indicating that the plasma implementation power and time cannot be too long.
[0129] The cyclic application experiment was carried out according to Application Example 10, and the difference from Application Example 10 was that the bouquet-shaped amorphous Co-PB alloy material I obtained in Example 2 was treated with low-temperature plasma. The power of the plasma generator was adjusted to 250 W, and the time was set to 600 s.
[0130] The catalytic experiment results show that compared with the catalytic performance of Example 10, which was significantly reduced after the 8th plasma treatment, the catalytic hydrogenation performance of the bouquet-shaped amorphous Co-PB alloy material II prepared in this comparative example has been significantly reduced after the 4th plasma treatment for the selective hydrogenation of furfural. The TEM test shows that the catalyst morphology has been largely destroyed. This shows that the plasma treatment power and time should not be too high or too long, otherwise it will be detrimental to the service life of the catalyst.
[0131] Table 1 Physicochemical properties of Co-PB nanomaterials
[0132]
Claims
1. A bouquet-shaped amorphous Co-PB alloy material, characterized in that: The invention has a micron-scale bouquet structure, wherein the micron-scale bouquet structure is assembled from a plurality of amorphous Co-PB alloy nanobelts.
2. The bouquet-shaped amorphous Co-PB alloy material according to claim 1, characterized in that: The amorphous Co-PB alloy nanobelt comprises the following molar percentage components: Co 65-69%; P 20~25%; B 10~11%。 3. The bouquet-shaped amorphous Co-PB alloy material according to claim 1 or 2, characterized in that: The amorphous Co-PB alloy nanobelt has a bandwidth of 80 to 300 nm; The overall length of the micrometer-scale bouquet structure is 2 to 6 μm, and the central angle is 45 to 160°.
4. The method for preparing a bouquet-shaped amorphous Co-PB alloy material according to any one of claims 1 to 3, characterized in that: The ligand and the cobalt salt are dissolved in water under the action of a surfactant to obtain a precursor solution; an alkaline solution containing sodium hypophosphite and sodium borohydride is added to the precursor solution to react to obtain a bouquet-shaped amorphous Co-PB alloy material I; or, the bouquet-shaped amorphous Co-PB alloy is further subjected to plasma treatment to obtain a bouquet-shaped amorphous Co-PB alloy material II.
5. The method for preparing a bouquet-shaped amorphous Co-PB alloy material according to claim 4, characterized in that: The mass ratio of the surfactant to the complexing agent is 6-8:0.5-1.2; The concentration of the cobalt salt is 0.1-1 mol / L.
6. The method for preparing a bouquet-shaped amorphous Co-PB alloy material according to claim 4 or 5, characterized in that: The cobalt salt includes cobalt chloride or a hydrate of cobalt chloride; The complexing agent includes D-(+) camphorsulfonic acid; The surfactant is Tween.
7. The method for preparing a bouquet-shaped amorphous Co-PB alloy material according to claim 4, characterized in that: The molar ratio of Co:P:B in the cobalt salt, sodium hypophosphite and sodium borohydride is controlled to be 1:(1-4):
2.
8. The method for preparing a bouquet-shaped amorphous Co-PB alloy material according to claim 3, characterized in that: The alkaline solution is pumped in at a speed of 0.05 to 0.10 mL / min.
9. The method for preparing a bouquet-shaped amorphous Co-PB alloy material according to claim 3, characterized in that: During the plasma treatment process, the power of the plasma generator is 150-200W, and the treatment time is 100-500s.
10. The use of a bouquet-shaped amorphous Co-PB alloy material according to claim 1 or 2, characterized in that: It is used as a catalyst for the hydrogenation of furfural to produce furfuryl alcohol.