Multi-power-source steel rail flash welding method

By introducing multi-power technology in rail welding, using the first electrode to heat the welding end face and the second electrode to heat the rail foot, the welding quality problem caused by uneven temperature is solved, the gray spot defect is eliminated, and the quality and quality of the welded joint are improved. Stability meets the fast-paced needs of modern railway construction.

CN118720376APending Publication Date: 2024-10-01METALS & CHEM RES INST CHINA ACAD OF RAILWAY SCI +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410707624.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional rail welding technology causes unstable welding quality due to uneven temperature when welding rail feet, and is prone to produce gray spot defects, which are difficult to detect through non-destructive testing and affect the quality and stability of the joints.

Method used

The multi-power rail flash welding method is adopted. The first electrode heats the welding end face, and the second electrode specifically heats the rail foot to ensure uniform current distribution, reduce gray spot defects, and improve the quality and stability of the welded joint.

Benefits of technology

It achieves uniform temperature distribution during the welding process, reduces gray spot defects, improves the quality and mechanical properties of welded joints, reduces maintenance and repair costs, enhances the safety and reliability of railway transportation, and improves welding operation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720376A_ABST
    Figure CN118720376A_ABST
Patent Text Reader

Abstract

The invention provides a multi-power-source steel rail flash welding method, and belongs to the technical field of steel rail welding. A first electrode is applied to the steel rail, and first voltage is loaded to the steel rail through the first electrode to heat the welding end face of the steel rail; applying a second electrode to the steel rail, loading a second voltage to the steel rail through the second electrode to heat a rail foot of the steel rail, and keeping the combined action of the first voltage and the second voltage until the welding end face of the steel rail flashes gently; and mechanical force pressure is applied to the end of the steel rail, and upsetting operation is completed. According to the multi-power-source steel rail flash welding method, the second power source is introduced to specially heat the rail bottom foot area, so that the distribution of current in the whole welding area is improved, the uniformity of the welding process is ensured, the welding quality problem caused by uneven current distribution is solved, the gray spot defect is reduced or even eliminated, and the welding quality is improved. The quality of the welding joint is improved, the maintenance and repair cost is reduced, the mechanical property of the welding joint is enhanced, and the safety and reliability of railway transportation are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rail welding, and in particular to a rail flash welding method. Background Art

[0002] Rail welding technology, as a core technology in the field of railway construction and maintenance, carries the important mission of ensuring the continuity, stability and safety of railway lines. With the continuous development of railway transportation, especially the rise of high-speed railways and heavy-duty railways, the requirements for rail welding technology are also increasing. This is not only because welding technology is directly related to the quality of railway lines, but also because it plays a vital role in ensuring the high-speed, stable and safe operation of trains.

[0003] The mainstream rail welding methods include flash welding, gas pressure welding and aluminothermic welding. Flash welding is widely favored for its high welding strength and smooth welding surface, and is particularly suitable for mass production in rail welding factories. Gas pressure welding uses the heat generated by gas combustion for welding, which is suitable for on-site operations at outdoor construction sites. Thermite welding uses high-temperature molten iron generated by thermite reaction to achieve rail connection. It is simple and convenient to operate and is particularly suitable for emergency repairs and other scenarios. Among these welding methods, flash welding has become the mainstream due to its high efficiency and automation. However, although the existing rail welding technology is quite mature, when facing some special parts, such as the welding of the rail foot, due to the complex shape of the rail foot, the traditional welding method often finds it difficult to ensure the uniform distribution of welding temperature, resulting in unstable welding quality. In addition, in the traditional rail welding technology, there are two main forms of electrode layout: one is to add electrodes to the waist of the rail, which is usually used for mobile welding machines; the other is to add electrodes to the rail bottom and rail head, which is suitable for fixed welding machines. Both layouts rely on a single power source for heating. However, due to the special profile of the rail foot, i.e., a thin plate-like structure, the temperature of the rail foot is relatively low when current passes through it under the same voltage conditions. This temperature unevenness will lead to an uneven flash process during welding, which in turn will produce a large beam explosion, providing conditions for the formation of gray spot defects. Gray spot defects are one of the most common problems in rail welded joints. It is not only difficult to detect through non-destructive testing methods, but also seriously affects the quality and stability of the welded joints. Therefore, there is an urgent need for efficient and high-quality welding technology in the field of railway construction. Summary of the invention

[0004] The purpose of the present invention is to propose a multi-power rail flash welding method, which improves the distribution of current during rail welding, especially increases the temperature of the rail foot area to ensure that the entire welding end face can be heated evenly, achieves a more uniform temperature distribution during the welding process, achieves uniform flash during the flash welding process, and thus eliminates uneven welding and gray spot defects caused by too low temperature in the rail foot area.

[0005] To achieve the above-mentioned object of the invention, the present invention provides a multi-power rail flash welding method, wherein a first electrode is applied to the rail, and a first voltage is applied to the rail through the first electrode to heat the welding end surface of the rail;

[0006] Applying a second electrode to the steel rail, applying a second voltage to the steel rail through the second electrode to heat the rail foot of the steel rail, and maintaining the first voltage and the second voltage acting together until the welding end surface of the steel rail flashes softly;

[0007] A mechanical force pressure is applied to the end of the rail to complete the upsetting operation.

[0008] Compared with the prior art, the present invention has the following characteristics and advantages:

[0009] The multi-power rail flash welding method proposed in the present invention introduces a second power source to heat the rail foot area specifically, thereby improving the distribution of current in the entire welding area and ensuring the uniformity of the welding process, so as to solve the welding quality problem caused by uneven current distribution, reduce or even eliminate gray spot defects, improve the quality of welded joints, reduce maintenance and repair costs, enhance the mechanical properties of welded joints, ensure the safety and reliability of railway transportation, and improve the efficiency of welding operations to meet the fast-paced requirements of modern railway construction. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] The accompanying drawings described herein are only for explanation purposes and are not intended to limit the scope of the present invention in any way. In addition, the shapes and proportional dimensions of the various components in the figures are only schematic, used to help understand the present invention, and are not specifically limited to the shapes and proportional dimensions of the various components of the present invention. Those skilled in the art can select various possible shapes and proportional dimensions to implement the present invention according to the teachings of the present invention.

[0011] Figure 1 It is a schematic diagram of the process flow of the multi-power rail flash welding method of the present invention;

[0012] Figure 2 A three-dimensional diagram of the loading positions of the first electrode and the second electrode in the present invention;

[0013] Figure 3 A three-dimensional top view of the loading positions of the first electrode and the second electrode in the present invention;

[0014] Figure 4 It is a schematic diagram of the second electrode wrapping the rail foot of the steel rail in the present invention;

[0015] Figure 5 This is a schematic diagram of a first electrode being loaded on both the rail bottom and the rail head in the present application;

[0016] Figure 6 is a schematic diagram of the rail temperature when only the first electrode is applied in this application;

[0017] Figure 7 This is a schematic diagram of the second electrode loading stage in this application.

[0018] Description of the accompanying drawings:

[0019] 10. Rail; 20. First electrode; 30. Second electrode;

[0021] a. The vertical distance between the geometric center of the first electrode and the welding surface;

[0022] b. The vertical distance from the geometric center of the second electrode to the welding surface. DETAILED DESCRIPTION

[0023] The details of the present invention can be more clearly understood with reference to the accompanying drawings and the description of the specific embodiments of the present invention. However, the specific embodiments of the present invention described herein are only used for the purpose of explaining the present invention and cannot be understood as limiting the present invention in any way. Under the guidance of the present invention, technicians can conceive of any possible variations based on the present invention, which should all be considered to belong to the scope of the present invention.

[0024] like Figure 1 As shown, the present invention proposes a multi-power rail flash welding method, wherein a first electrode is applied to the rail, and a first voltage is applied to the rail through the first electrode to heat the welding end surface of the rail;

[0025] Applying a second electrode to the steel rail, applying a second voltage to the steel rail through the second electrode to heat the rail foot of the steel rail, and maintaining the first voltage and the second voltage acting together until the flash of the welded end face of the steel rail is soft;

[0026] Apply mechanical pressure to the rail ends and complete the upsetting operation.

[0027] In the multi-power rail flash welding method proposed by the present invention, the first electrode mainly heats the welding end face of the rail to form a suitable upsetting temperature field. The second electrode mainly applies voltage to the rail foot to destroy the lintel explosion of the rail foot adhesion part through the current, thereby reducing the intensity of the rail foot flash and making the flash more uniform. Finally, the gray spot defect loses the formation conditions and eliminates the gray spot defect.

[0028] The multi-power rail flash welding method proposed by the present invention introduces a second electrode to heat the rail foot area specifically, thereby improving the distribution of current in the entire welding area, ensuring the uniformity of the welding process, solving the welding quality problem caused by uneven current distribution, reducing or even eliminating gray spot defects, improving the quality of the welded joint, reducing maintenance and repair costs, enhancing the mechanical properties of the welded joint, ensuring the safety and reliability of railway transportation, and improving the efficiency of welding operations, meeting the fast-paced requirements of modern railway construction. In an optional embodiment of the present invention, when the first electrode 20 loads the first voltage to the rail, the second electrode 30 synchronously loads the second voltage. The first electrode 20 first applies a voltage to the rail 10 to heat the end of the rail 10 to a near-molten state. After the first voltage loading lasts for a predetermined time, usually a time period pre-set according to the material of the rail and the required welding temperature, the second electrode begins to apply the second voltage to the foot area of ​​the rail 10. This synchronous voltage loading operation ensures the uniform distribution of current and heat during the welding process, and effectively avoids the problem of local overheating or uneven welding caused by current concentration.

[0029] In an optional embodiment of the present invention, after the first voltage is applied for a predetermined time, the second electrode 30 applies the second voltage to the rail 10 .

[0030] In an optional example of this embodiment, after the first electrode 20 applies a first voltage to the steel rail 10 until the end of the burning period, the second electrode 30 applies a second voltage to the steel rail 10 .

[0031] Specifically, the first electrode 20 applies a first voltage to the rail 10, so that the end of the rail 10 is heated to a state close to melting, and the time is pre-set. Subsequently, when the welding process enters the final stage of the burning process, that is, when the material at the end of the rail 10 is close to being completely melted and before the upsetting operation, the second electrode 30 begins to apply a second voltage to the rail foot area of ​​the rail 10. The implementation method of applying voltage in stages in this embodiment can ensure that the rail foot area is properly heated in the later stage of the welding burning stage by accurately controlling the loading timing of the second voltage, effectively improving the overall temperature uniformity of the welded joint, and avoiding local overheating or uneven welding. Secondly, by optimizing the temperature distribution and melting during the welding process through this method, it is possible to improve welding efficiency and productivity, significantly improve the quality of the welded joint, extend the service life of the rail, and reduce energy consumption.

[0032] In an optional embodiment of the present invention, the soft flash of the welding end face means that the flash current exceeds 30% to 50% of the average current peak value. By applying the second voltage, the current parameters in the welding process can be more accurately controlled to achieve soft flash of the welding end face.

[0033] Furthermore, during the welding process, by adjusting the first voltage and the second voltage, welding parameters such as current, voltage, and frequency can also be adjusted so that the peak value of the flash current exceeds 30% to 50% of the average current, so as to ensure that the flash of the welding end face is neither too intense nor too weak, but in a gentle state. This gentle state of the flash of the welding end face helps to ensure the quality of the welded joint, so that the melting and bonding during the welding process are carried out under controlled conditions, reducing the risk of over-melting due to excessive current or insufficient welding due to too low current.

[0034] In an optional embodiment of the present invention, the first electrode 20 is applied to the rail head, rail web and / or rail bottom of the rail 10 .

[0035] In an optional example of this embodiment, a vertical distance a between the geometric center of the first electrode 20 and the welding surface is 100 mm to 300 mm.

[0036] Specifically, the first electrode 20 can be applied to the waist or bottom of the rail 10, and the vertical distance between the first electrode 20 and the welding surface can be controlled to be between 100 mm and 300 mm, which can ensure the uniform distribution of current and effective heating during the welding process, thereby improving the quality and consistency of the welded joint. This precise electrode position control helps to reduce welding defects such as unwelded, slag inclusion or overburning, and can also improve the stability of the welding process, making welding parameters easier to control, thereby maintaining the consistency of welding quality in large-scale production, significantly improving welding efficiency, reducing production costs, and improving the reliability and durability of welded joints.

[0037] In an optional example of this embodiment, Figure 2 As shown, the first electrode is applied only at the rail head.

[0038] In another optional example of this embodiment, the first electrode is applied only at the web of the rail.

[0039] In another optional example of this embodiment, Figure 5 As shown, first electrodes are applied respectively at the rail head and rail foot of the rail.

[0040] In an optional embodiment of the present invention, the second electrode 30 is applied to the foot of the rail 10. The second electrode 30 is applied to the foot region of the rail 10, which solves the problem of uneven welding and low temperature caused by insufficient current density at the foot of the rail in the prior art. During the welding process, after the first electrode 20 applies voltage to the rail waist or rail bottom for preliminary heating, the activation of the second electrode 30 further heats the foot region in a targeted manner, so that the current flows more concentratedly to the foot of the rail, thereby increasing the temperature of the region, ensuring that the melting and bonding during the welding process are more complete and uniform.

[0041] In an optional example of this embodiment, the vertical distance b between the geometric center of the second electrode 30 and the welding surface is 20 mm to 100 mm. Specifically, the specific position where the second electrode 30 is placed strictly controls the vertical distance between the geometric center of the second electrode 30 and the welding surface within the range of 20 mm to 100 mm. This distance can ensure that the rail foot area is evenly and appropriately heated, thereby improving the overall quality and consistency of the welded joint.

[0042] In an optional example of this embodiment, the second electrode 30 is wrapped around the bottom of the rail foot. The layout of the second electrode 30 wrapped around the bottom of the rail foot of the rail 10 allows the second electrode 30 to contact the rail foot area more closely, thereby providing more concentrated and effective heating during the welding process, helping to ensure the temperature uniformity of the area during the welding process, thereby reducing the risk of uneven welding and defects.

[0043] In an optional embodiment of the present invention, a first voltage is applied to the rail to be welded, and the first electrode 20 is the main heating power source, and the second electrode 30 is applied when entering the late stage of burning. The application positions of the first electrode 20 and the second electrode 30 are different. The first electrode 20 is applied to the rail waist or rail head. The second electrode 30 is applied to the rail foot. The vertical distance a from the geometric center of the first electrode 20 to the welding surface is 100mm to 300mm, and the vertical distance b from the geometric center of the second electrode 30 to the welding surface is 20mm to 100mm. The first electrode is in a fixed position, and the second electrode 30 can adjust the vertical distance from the welding surface. Furthermore, the actual distance of the second electrode 30 is determined according to the consumed length of the rail, which is usually 10mm to 50mm larger than the consumed length of the rail.

[0044] In an optional embodiment of the present invention, the first electrode 20 is connected to a first power supply, which is a DC power supply or an AC power supply, and the second electrode 30 is connected to a second power supply, which is a DC power supply or an AC power supply. The first electrode 20 is connected to a first power supply, which can be selected as a DC power supply or an AC power supply, which is determined according to actual application requirements and circuit design. Similarly, the second electrode 30 is connected to a second power supply, which can also be a DC power supply or an AC power supply. Such a design provides flexibility in power supply selection, so that the circuit system can adapt to different working environments and power supply conditions. In actual operation, if a stable current supply is required, a DC power supply can be selected; and in certain specific scenarios, such as when the characteristics of AC power need to be utilized, an AC power supply can be selected. The two power supplies can be selected and controlled independently, and the most suitable power supply type can be selected according to different welding conditions and rail material characteristics, thereby improving the quality of the welded joint and the stability of the welding process. The multi-power supply configuration of the present invention can help optimize the temperature control and heat-affected zone management during welding, further improve welding efficiency and reduce energy consumption.

[0045] In an optional example of this embodiment, the output power of the second power supply is dynamic power. The output power of the second power supply is designed to be dynamically adjustable and can be adjusted in real time according to the actual needs of the welding process, and is not constant. Dynamic power adjustment can ensure uniform distribution of heat during welding, especially in the rail foot area of ​​the rail 10, which helps to avoid welding defects caused by uneven heat distribution, such as gray spots and unwelded joints. This dynamic adjustment capability makes the welding process more flexible and responsive, and the power output can be adjusted in time according to changes in welding conditions, thereby improving welding efficiency and the quality of welded joints.

[0046] The main function of the first electrode 20 is to heat the welding end face to form a suitable upsetting temperature field. The main function of the second electrode 30 is to apply voltage to the rail foot during the final burning so that the beam explosion of the rail foot adhesion part passing through the current is destroyed. As a result, the flash intensity of the rail foot is reduced and the flash is more uniform. As a result, the gray spot defect loses the formation conditions and eliminates the gray spot defect.

[0047] In another optional example of this implementation, the output power of the second power supply is constant power.

[0048] In an optional example of this embodiment, the output power of the second electrode 30 is 0% to 30% of the output power of the first electrode 20. In the method of the present invention, the output power of the second electrode 30 can be finely controlled. By adjusting the power output of the second electrode 30, the heat input at the welding end face, especially at the rail foot, can be accurately controlled to ensure thermal balance during welding. Through in-depth research and experimental verification of the welding process, it is found that its value is set within the range of 0% to 30% of the output power of the first electrode 20. The setting of this power ratio helps to achieve temperature uniformity during welding, especially in the rail foot area, thereby effectively preventing the generation of uneven welding and welding defects. Secondly, by accurately controlling the power output of the second electrode 30, the microstructure and mechanical properties of the welded joint can be optimized, and the overall quality of the welded joint can be improved. In addition, this power control strategy also helps to improve the stability and repeatability of the welding process, making the welding parameters easier to control and suitable for large-scale production environments. In an optional embodiment of the present invention, after the top forging operation is completed, the rail is pushed to improve the flatness of the welded joint.

[0049] The specific implementation process of the present invention is now described in detail with reference to the embodiments:

[0050] Step 1: Applying the first electrode 20

[0051] The end surface of the rail 10 begins to heat up under the action of the first electrode 20, and the first electrode 20 is attached to the head and the bottom of the rail 10. However, the heating of the first electrode 20 will cause the temperature of the rail bottom to be low, such as Figure 6 shown.

[0052] Step 2: In the late stage of burning, apply the second electrode 30 to the rail foot

[0053] The stage of applying the second electrode 30 is shown in 7. When the welding stage enters the burning stage, the second electrode 30 is loaded. The fitting position and shape characteristics of the first electrode 20 and the second electrode 30 are as follows: Figures 2 to 4 The second electrode 30 is wrapped around the rail foot. The geometric relationship of the second electrode 30 on the rail 10 is as shown in FIG. Figure 5 shown.

[0054] The output power of the second electrode 30 is dynamic power. Its power is 0% to 30% of the first electrode 20, which is related to the flashing degree of the rail foot. When the flashing at the rail foot is intense and uneven, the power increases until the flashing is uniform.

[0055] Step 4: Upsetting with electricity

[0056] The first electrode 20 and the second electrode 30 work together to complete the charged upsetting.

[0057] The dual-power source welding method for rail welding provided by the present invention eliminates inherent gray spots compared to the existing rail welding process.

[0058] In this embodiment, 15 rail joints were welded by the dual power welding method. After the drop hammer test, the fracture gray spot area was counted. It can be seen that the dual power welding method greatly reduced more than 99% of the joint gray spot defects, as shown in Table 1.

[0059] Table 1

[0060]

[0061]

[0062] The detailed explanation of the above-mentioned embodiments is only intended to explain the present invention so as to facilitate a better understanding of the present invention. However, these descriptions cannot be interpreted as limitations on the present invention for any reason. In particular, the various features described in different embodiments may also be arbitrarily combined with each other to form other embodiments. Unless there is a clear description to the contrary, these features should be understood to be applicable to any embodiment and are not limited to the described embodiments.

Claims

1. A multi-power rail flash welding method, characterized in that: The welding method comprises: Applying a first electrode to the steel rail, and applying a first voltage to the steel rail through the first electrode to heat the welding end surface of the steel rail; Applying a second electrode to the steel rail, applying a second voltage to the steel rail through the second electrode to heat the rail foot of the steel rail, and maintaining the first voltage and the second voltage acting together until the flash of the welding end face of the steel rail is soft; A mechanical force pressure is applied to the end of the rail to complete the upsetting operation.

2. The multi-power rail flash welding method according to claim 1, characterized in that: When the first electrode applies the first voltage to the rail, the second electrode is synchronously applied with a second voltage.

3. The multi-power rail flash welding method according to claim 1, characterized in that: After the first voltage is applied for a predetermined time, the second electrode applies the second voltage to the rail.

4. The multi-power rail flash welding method according to claim 3, characterized in that: After the first electrode applies the first power to the rail until the end of the burning, the second electrode applies the second voltage to the rail.

5. The multi-power rail flash welding method according to claim 1, characterized in that: The soft flash of the welding end face means that the flash current exceeds 30% to 50% of the average current peak value.

6. The multi-power rail flash welding method according to claim 1, characterized in that: The first electrode is applied to the rail head, rail web and / or rail bottom of the rail.

7. The multi-power rail flash welding method according to claim 6, characterized in that: The vertical distance between the geometric center of the first electrode and the welding surface is 100 mm to 300 mm.

8. The multi-power rail flash welding method according to claim 1, characterized in that: The second electrode is applied to the rail foot of the rail.

9. The multi-power rail flash welding method according to claim 9, characterized in that: The vertical distance between the geometric center of the second electrode and the welding surface is 20 mm to 100 mm.

10. The multi-power rail flash welding method according to claim 9, characterized in that: The second electrode is wrapped around the bottom of the rail foot.

11. The multi-power rail flash welding method according to claim 1, characterized in that: The first electrode is connected to a first power source, which is a DC power source or an AC power source, and the second electrode is connected to a second power source, which is a DC power source or an AC power source.

12. The multi-power rail flash welding method according to claim 11, characterized in that: The output power of the second power supply is dynamic power.

13. The power rail flash welding method according to claim 12, characterized in that: The output power of the second power supply is 0% to 30% of the output power of the first power supply.

Citation Information

Cited By

  • Constant displacement control method for steel rail flash welding

    CN120269336A