Low-temperature solder and preparation method and application thereof

By adding zinc and rare earth elements to the low-temperature solder, the growth of IMC is suppressed and the mechanical properties are improved. The problem of IMC growth in high-temperature environments in the existing technology is solved, and the stability of the photovoltaic cell module and the strength of the solder joints are improved.

CN118720519APending Publication Date: 2024-10-01TRINA SOLAR CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411108522.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing low-temperature solders lead to the growth of intermetallic compounds (IMC) in high-temperature environments, affecting the long-term stability of components and the mechanical properties of solder joints.

Method used

Add 0.1-1.5% zinc and 0.05-0.2% rare earth elements to the low-temperature solder to form a ZnAg alloy, which increases the activation energy of self-diffusion of tin and silver elements, inhibits IMC growth, and hinders further IMC growth through physical adsorption of rare earth elements. , improve the mechanical properties of solder.

Benefits of technology

It effectively inhibits the growth of IMC, improves the mechanical properties of solder joints and the long-term stability of components, and increases the tensile force value of photovoltaic cells after string welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720519A_ABST
    Figure CN118720519A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a low-temperature solder and a preparation method and application thereof, and the low-temperature solder comprises the following components in percentage by mass: 14-26% of bismuth, 37-43% of lead, 0.1-1.5% of zinc, 0.05-0.2% of rare earth element and the balance of tin based on 100% of the total mass of the low-temperature solder. According to the low-temperature solder, zinc and rare earth elements with specific contents are added into the low-temperature solder, so that zinc and silver can form ZnAg alloy in the welding process of the solder, the activation energy during subsequent tin and silver element self-diffusion is increased, the difficulty of SnAg metallization formation is increased, the growth of welding spot IMC is inhibited, the rare earth elements can be physically adsorbed on the surface of the formed IMC, and the welding quality of the solder is improved. Further growth of IMC is hindered and inhibited; in addition, through the synergistic effect of rare earth elements and zinc, the mechanical property of the solder can be effectively enhanced, and the tension value of photovoltaic cells after series welding is effectively increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a low-temperature solder and a preparation method and application thereof. Background Art

[0002] At present, low-temperature solder strips are used for string welding of heterojunction photovoltaic cells. The components of the surface coating of the low-temperature solder strips (i.e., low-temperature solder) after string welding are Bi-14wt%, Sn-43wt%, and Pb-wt43%. After welding, the tin in the low-temperature solder will form an intermetallic compound (IMC) with the silver in the paste on the surface of the cell, namely Ag3Sn, which is also the basis for the effective connection between the solder strip and the cell.

[0003] However, IMC will grow in high-temperature environments such as component lamination and hot spots. When the thickness of IMC exceeds a certain thickness, there is a risk of IMC cracking, which will seriously affect the stability of the component during long-term use.

[0004] In addition, since the mechanical properties of the coating on the surface of the solder strip after welding with the low-temperature solder used in the above-mentioned heterojunction battery are low, the tensile force value of the solder joint after string welding is low, and a large part of the reason is the fracture at the solder.

[0005] In view of the problems existing in the existing technology, a new type of low-temperature solder has been developed. On the basis of ensuring the mechanical properties of the solder strip, it can also effectively inhibit the growth of IMC and ensure the stability of the components during long-term use. Summary of the invention

[0006] The embodiments of the present application provide a low-temperature solder and a preparation method and application thereof to solve or alleviate at least one of the technical problems mentioned above.

[0007] In a first aspect, an embodiment of the present application provides a low-temperature solder, which includes 14-26% by weight of bismuth, 37-43% by weight of lead, 0.1-1.5% by weight of zinc, 0.05-0.2% by weight of rare earth elements, and the remainder of tin, based on the total weight of the low-temperature solder being 100%.

[0008] Optionally, the ratio of the added amount of zinc to the rare earth element is (7.5-10):1.

[0009] Optionally, the rare earth element includes any one of cerium, lanthanum, or neodymium, or a combination of at least two of them.

[0010] Optionally, when the rare earth element is cerium, the added amount of cerium is 0.08-0.12%.

[0011] Optionally, when the rare earth element is lanthanum, the added amount of lanthanum is 0.1-0.15%.

[0012] Optionally, when the rare earth element is neodymium, the added amount of neodymium is 0.13-0.16%.

[0013] In a second aspect, an embodiment of the present application provides a low-temperature solder, and a method for preparing the low-temperature solder includes:

[0014] Bismuth with a mass percentage of 14-26%, lead with a mass percentage of 37-43% and the balance of tin are melt-mixed at 400-500° C. for 30-60 minutes, and then zinc with a mass percentage of 0.1-1.5% and rare earth elements with a mass percentage of 0.05-0.2% are added and melt-mixed for a second time at 400-500° C. for 60-120 minutes to obtain the low-temperature solder.

[0015] Optionally, during the preparation of the low-temperature solder, a eutectic salt of potassium chloride and lithium chloride in a mass ratio of (1-1.5):1 is used to cover the solder surface to protect it;

[0016] After the secondary melt mixing is uniform, the eutectic salt on the surface of the molten mixture is removed.

[0017] Optionally, the method further comprises: performing cold casting after the secondary melt mixing.

[0018] In a third aspect, an embodiment of the present application provides an application of a low-temperature solder in the processing of photovoltaic modules.

[0019] The technical solution adopted in the embodiment of the present application may include the following advantages: by adding 0.1-1.5% by weight of zinc and 0.05-0.2% by weight of rare earth elements to the low-temperature solder, zinc can form a ZnAg alloy with silver during the soldering process, thereby increasing the activation energy of subsequent self-diffusion of tin and silver elements, increasing the difficulty of SnAg metallization formation, and inhibiting the growth of IMC at the solder joint, and the rare earth elements can be physically adsorbed on the surface of the formed IMC, hindering and inhibiting the further growth of the IMC; in addition, through the synergistic effect of rare earth elements and zinc, the mechanical properties of the solder can be effectively enhanced, and the tensile force value of the photovoltaic cells after string welding is effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0021] Figure 1 This is a scanning electron microscope image of the low-temperature solder prepared in Example 1, with a scale of 10 μm.

[0022] Figure 2This is a scanning electron microscope image of the low-temperature solder prepared in Comparative Example 1, with a scale of 10 μm.

[0023] Figure 3 The metallographic images of the low-temperature solder prepared in Example 1 after welding and after treatment at 200°C for 2h;

[0024] Figure 4 The metallographic images of the low-temperature solder prepared in Comparative Example 1 after welding and after treatment at 200°C for 2h;

[0025] Figure 5 This is a comparison chart of the mechanical properties of the low-temperature solders prepared in Example 1 and Comparative Example 1 after forming solder strips;

[0026] Figure 6 The metallographic images of the low-temperature solder prepared in Comparative Example 2 after welding and after treatment at 200°C for 2h;

[0027] Figure 7 The metallographic images of the low-temperature solder prepared in Comparative Example 3 after welding and after treatment at 200°C for 2h;

[0028] Figure 8 The metallographic images of the low-temperature solder prepared in Example 4 after welding and treatment at 200°C for 2h;

[0029] Fig. 9 The metallographic images of the low-temperature solder prepared in Example 6 after welding and treatment at 200°C for 2h;

[0030] Fig.10 The metallographic images of the low-temperature solder prepared in Example 8 after welding and after treatment at 200°C for 2h;

[0031] Fig.11 This is the metallographic image of the low-temperature solder prepared in Example 11 after welding and treatment at 200°C for 2h. DETAILED DESCRIPTION

[0032] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.

[0033] The present application provides a low-temperature solder, which, based on the total mass of the low-temperature solder being 100%, comprises 14-26% by mass (exemplarily, the mass percentage of bismuth is 14%, 16%, 18%, 20%, 22%, 24%, 26%, etc.) of bismuth, 37-43% (exemplarily, the mass percentage of lead is 37%, 38%, 39%, 40%, 41%, 42%, 43% of lead, etc.) of tantalum. % etc.) of lead, 0.1-1.5% (exemplarily, the mass percentage of lead is 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5% etc.) of zinc, 0.05-0.2% (exemplarily, the mass percentage of rare earth elements is 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18%, 0.2% etc.) of rare earth elements and the balance of tin.

[0034] It should be noted that low-temperature solder refers to adding bismuth to conventional tin-lead solder, so that the melting point of the solder is lower than that of conventional tin-lead solder (melting point is 183°C), so it is called low-temperature solder. The basic composition of the solder in the embodiment of the present application is tin, lead and bismuth, and a small amount or trace amount of zinc and rare earth elements are added thereto, which has little effect on the melting point of the solder as a whole, so that its melting point is still lower than that of conventional tin-lead solder, and therefore it belongs to low-temperature solder.

[0035] In low temperature solder, the role and function of each component are as follows:

[0036] The role of bismuth in low-temperature solder is to lower the melting point of the solder.

[0037] The role of lead in low-temperature solder is to reduce the surface tension of the molten solder and increase its wetting and spreading on the silver electrode.

[0038] The role of tin in low-temperature solder is to form a metallurgical bond with the silver electrode, which determines the strength and reliability of the solder joint.

[0039] The role of zinc in low-temperature solder is: it can form an alloy with silver during the welding process, increase the difficulty of tin and silver forming an alloy, thereby inhibiting the growth of IMC in the solder joint and increasing the mechanical properties of the solder joint.

[0040] The role of rare earth elements in low-temperature solders is to work synergistically with zinc to inhibit IMC growth and increase the mechanical properties of the solder joints.

[0041] By creatively adding specific amounts of zinc and rare earth elements to low-temperature solder, zinc can form a ZnAg alloy with silver during the soldering process, increasing the activation energy of subsequent self-diffusion of tin and silver elements, increasing the difficulty of SnAg metallization formation, and inhibiting the growth of IMC in solder joints. Rare earth elements can be physically adsorbed on the surface of the already formed IMC, hindering and inhibiting the further growth of IMC. In addition, the synergistic effect of rare earth elements and zinc can effectively enhance the mechanical properties of the solder, which is beneficial to effectively improve the tensile force value of photovoltaic cells after string soldering.

[0042] In some embodiments, the ratio of the amount of zinc added to the rare earth element is (7.5-10):1, and illustratively, the ratio of the amount of zinc added to the rare earth element is 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1, etc. When the ratio of the amount of zinc added to the rare earth element is (7.5-10):1, on the basis of ensuring that the melting point of the low-temperature solder changes little, the growth of IMC can be better inhibited and the mechanical properties of the solder can be increased.

[0043] In some embodiments, the rare earth element includes any one or a combination of at least two of cerium, lanthanum, or neodymium.

[0044] In some embodiments, when the rare earth element is cerium, the amount of cerium added is 0.08-0.12% (exemplarily, the amount of cerium added is 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, etc.). When the rare earth element is specifically selected as cerium, adding 0.08-0.12% can better synergize with zinc to inhibit IMC growth and increase the mechanical properties of the solder.

[0045] In some embodiments, when the rare earth element is lanthanum, the amount of lanthanum added is 0.1-0.15% (exemplarily, the amount of lanthanum added is 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, etc.). When lanthanum is specifically selected as the rare earth element, adding 0.1-0.15% can better synergize with zinc to inhibit IMC growth and increase the mechanical properties of the solder.

[0046] In some embodiments, when the rare earth element is neodymium, the amount of neodymium added is 0.13-0.16% (exemplarily, the amount of neodymium added is 0.13%, 0.14%, 0.15%, 0.16%, etc.). When neodymium is specifically selected as the rare earth element, adding 0.13-0.16% can better synergize with zinc to inhibit IMC growth and increase the mechanical properties of the solder.

[0047] The present application provides a method for preparing a low-temperature solder, comprising:

[0048] Bismuth with a mass percentage of 14-26%, lead with a mass percentage of 37-43%, and the remainder of tin are melt-mixed at 400-500°C (exemplarily, the temperature is 400°C, 420°C, 450°C, 470°C, 500°C, etc.) for 30-60 min (exemplarily, the mixing time is 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.), and then zinc with a mass percentage of 0.1-1.5% and rare earth elements with a mass percentage of 0.05-0.2% are added and melt-mixed for a second time at 400-500°C (exemplarily, the temperature is 400°C, 420°C, 450°C, 470°C, 500°C, etc.) for 60-120 min (exemplarily, the mixing time is 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, etc.) to obtain a low-temperature solder.

[0049] In some embodiments, during the preparation of the low-temperature solder, a eutectic salt of potassium chloride and lithium chloride in a mass ratio of (1-1.5):1 (exemplarily, the mass ratio of potassium chloride to lithium chloride is 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, etc.) is used to cover the surface of the solder to protect it and prevent the metal elements from being oxidized; after the secondary melt mixing is uniform, the eutectic salt on the surface of the molten mixture is removed.

[0050] In some embodiments, the preparation method further comprises performing cold casting after the secondary melt mixing.

[0051] The following specific examples further illustrate the present application, but should not be construed as limiting the present application. Without departing from the spirit and substance of the present application, modifications or replacements made to the methods, steps or conditions of the present application are within the scope of the present application.

[0052] In heterojunction cells, the composition of the commonly used low-temperature solder is: 14-26% bismuth, 37-43% lead and the balance of tin. Through the solder composition within this content range, 0.1-1.5% zinc and 0.05-0.2% rare earth elements were used for experiments. It was found that when the bismuth content was 14%, the tin content was 43%, and the lead content was 43%, the performance of the heterojunction battery in subsequent processing and use would be better. Therefore, the embodiment of the present application is adjusted on the basis of the optimal composition of the conventional solder, and the growth and further growth of the IMC are further suppressed on the basis of not changing the performance of the original solder as much as possible, and the mechanical properties of the solder alloy are further increased.

[0053] [Example 1]

[0054] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 41.9% by weight of tin, 1% by weight of zinc and 0.1% by weight of rare earth element cerium, wherein the ratio of the added amounts of zinc to cerium is 10:1.

[0055] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0056] 14% bismuth, 43% lead and 41.9% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1% zinc and 0.1% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0057] [Comparative Example 1]

[0058] This comparative example provides a low-temperature solder, which includes 14% by mass of bismuth, 43% by mass of lead and 43% by mass of tin.

[0059] This comparative example also provides a method for preparing a low-temperature solder, comprising:

[0060] 14% bismuth, 43% lead and 43% tin by mass are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0061] Figure 1 This is the morphology of the low-temperature solder prepared in Example 1. Figure 2 This is a morphology diagram of the low-temperature solder prepared in Comparative Example 1. By comparison, it is found that the low-temperature solder prepared in Example 1 has a finer alloy structure than the low-temperature solder prepared in Comparative Example 1.

[0062] The low-temperature solders prepared in Example 1 and Comparative Example 1 were sampled and placed at 200°C for 2 hours (simulating the solder joint being in an extreme hot spot environment). The metallographic images of the treated low-temperature solders were observed. Figure 3 and Figure 4 , Figure 3 The metallographic image of the solder prepared in Example 1 after high temperature treatment. Figure 4 For comparative example, the metallographic image of the solder after high temperature treatment was obtained by Figure 3 and Figure 4Comparison shows that the size and growth range of the intermetallic compound IMC of the low-temperature solder of Example 1 after high-temperature treatment are much lower than those of Comparative Example 1.

[0063] The solders obtained in Example 1 and Comparative Example 1 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Example 1 was 35.7 MPa, the Young's modulus was 18.5 MPa, and the tensile strength was 52.2 MPa. The yield strength obtained by the tensile test of the solder prepared in Comparative Example 1 was 32.2 MPa, the Young's modulus was 16.2 MPa, and the tensile strength was 48.1 MPa. The comparison results of the tensile test are shown in FIG. Figure 5 It can be found that the tensile strength, yield strength and Young's modulus of the alloy of the low-temperature solder prepared in Example 1 are significantly higher than the alloy strength of the low-temperature solder prepared in Comparative Example 1.

[0064] [Comparative Example 2]

[0065] This comparative example provides a low-temperature solder, which includes 14% by mass of bismuth, 43% by mass of lead, 1.1% by mass of zinc and 41.9% by mass of tin.

[0066] This comparative example also provides a method for preparing a low-temperature solder, comprising:

[0067] 14% bismuth, 43% lead and 41.9% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.1% zinc is added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold cast in a mold to form a low-temperature solder.

[0068] [Comparative Example 3]

[0069] This comparative example provides a low-temperature solder, which includes 14% by mass of bismuth, 43% by mass of lead, 0.1% by mass of a rare earth element (cerium), and 42.9% by mass of tin.

[0070] This comparative example also provides a method for preparing a low-temperature solder, comprising:

[0071] 14% bismuth, 43% lead and 42.9% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 0.1% rare earth element (cerium) is added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0072] Comparative Examples 2 and 3 were subjected to the same morphology test as Example 1, and it was found that Example 1 had the finest and densest structure, and the particle sizes of the structures of Comparative Examples 2 and 3 were significantly larger than those of Example 1.

[0073] Figure 6 The metallographic images of the low-temperature solder prepared in Comparative Example 2 after welding and after treatment at 200°C for 2h are shown below. Figure 7 This is a metallographic image of the low-temperature solder prepared in Comparative Example 3 after welding and treatment at 200°C for 2h. By comparing with Example 1, it is found that the IMC growth thickness of the solders prepared in Comparative Examples 2 and 3 after welding and treatment at 200°C for 2h is significantly thicker than that of Example 1, indicating that the solder must contain both zinc and the rare earth element cerium, and the synergistic effect of the two can have a better inhibitory effect on IMC growth.

[0074] The solders obtained in Comparative Examples 2 and 3 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Comparative Example 2 was 34.9 MPa, the Young's modulus was 18.2 MPa, and the tensile strength was 48.1 MPa. The yield strength obtained by the tensile test of the solder prepared in Comparative Example 3 was 32.3 MPa, the Young's modulus was 16.72 MPa, and the tensile strength was 45 MPa. By comparing Example 1 with Comparative Examples 2-3, it can be seen that the tensile strength, yield strength and Young's modulus of the alloy of the low-temperature solder prepared in Example 1 are significantly higher than the alloy strength of the low-temperature solder prepared in Comparative Examples 2-3.

[0075] [Example 2]

[0076] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 41.98% by weight of tin, 0.9% by weight of zinc and 0.12% by weight of the rare earth element cerium, wherein the ratio of the added amounts of zinc to cerium is 7.5:1.

[0077] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0078] 14% bismuth, 43% lead and 41.98% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 0.9% zinc and 0.12% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0079] [Example 3]

[0080] The present embodiment provides a low-temperature solder, including 14% by weight of bismuth, 43% by weight of lead, 42.2% by weight of tin, 0.72% by weight of zinc, and 0.08% by weight of rare earth element cerium, wherein the mass ratio of zinc to cerium is 9:1.

[0081] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0082] 14% bismuth, 43% lead and 42.2% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 0.72% zinc and 0.08% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0083] By performing the same morphology test on Example 2 and Example 3 as that on Example 1, the test results are similar, and they also have fine alloy structures.

[0084] The solders obtained in Example 2 and Example 3 were subjected to metallographic testing after high temperature treatment, and it was found that the IMC size and growth range of the intermetallic compounds of the low-temperature solders in Example 2 and Example 3 after high temperature treatment were similar to those in Example 1.

[0085] The solders obtained in Examples 2 and 3 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Example 2 was 35.4 MPa, the Young's modulus was 18.8 MPa, and the tensile strength was 52 MPa. The yield strength obtained by the tensile test of the solder prepared in Example 3 was 35.9 MPa, the Young's modulus was 18 MPa, and the tensile strength was 52.4 MPa, indicating that the solders prepared in Examples 2-3 have good mechanical properties.

[0086] [Example 4]

[0087] The present embodiment provides a low-temperature solder, including 14% by weight of bismuth, 43% by weight of lead, 41.72% by weight of tin, 1.2% by weight of zinc, and 0.08% by weight of the rare earth element cerium, wherein the mass ratio of zinc to cerium is 15:1.

[0088] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0089] 14% bismuth, 43% lead and 41.72% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.2% zinc and 0.08% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0090] [Example 5]

[0091] The present embodiment provides a low-temperature solder, including 14% by weight of bismuth, 43% by weight of lead, 41.4% by weight of tin, 0.5% by weight of zinc, and 0.1% by weight of the rare earth element cerium, wherein the mass ratio of zinc to cerium is 5:1.

[0092] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0093] 14% bismuth, 43% lead and 41.4% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 0.5% zinc and 0.1% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0094] By performing the same morphology test on Example 4 and Example 5 as that on Example 1, the test results are similar, and both have fine alloy structures, but the density is slightly lower than that of Example 1.

[0095] Figure 8 The metallographic diagram of the solder obtained in Example 4 after high temperature treatment shows that the IMC size and growth range of the intermetallic compound of the low-temperature solder prepared in Example 4 after high temperature treatment are slightly worse than those in Example 1. The metallographic diagram of the solder obtained in Example 5 after high temperature treatment is tested, and the results are similar to those in Example 4.

[0096] The solders obtained in Examples 4 and 5 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Example 4 was 30.3 MPa, the Young's modulus was 21.2 MPa, and the tensile strength was 53 MPa. The yield strength obtained by the tensile test of the solder prepared in Example 5 was 31.2 MPa, the Young's modulus was 20.8 MPa, and the tensile strength was 52.4 MPa, indicating that the solders prepared in Examples 4-5 have good mechanical properties.

[0097] By comparing Example 1 with Examples 4-5, it can be seen that when the addition amounts of zinc and cerium are not within the most preferred range of the present application, the ability to inhibit the growth of IMC and inhibit further growth of IMC is slightly poor, and further improvement of mechanical properties will be affected.

[0098] [Example 6]

[0099] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 41.35% by weight of tin, 1.5% by weight of zinc and 0.15% by weight of the rare earth element cerium, wherein the mass ratio of zinc to cerium is 10:1.

[0100] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0101] 14% bismuth, 43% lead and 41.35% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.5% zinc and 0.15% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0102] [Example 7]

[0103] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 41.95% by weight of tin, 1% by weight of zinc, and 0.05% by weight of the rare earth element cerium, wherein the mass ratio of zinc to cerium is 20:1.

[0104] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0105] 14% bismuth, 43% lead and 41.95% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1% zinc and 0.05% rare earth element (cerium) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0106] By performing the same morphology test as Example 1 on Example 6 and Example 7, the test results are similar, and they also have fine alloy structures, but the density is slightly worse than that of Example 1.

[0107] Fig. 9 The metallographic image of the solder obtained in Example 6 after high temperature treatment shows that the IMC size and growth range of the intermetallic compound of the low-temperature solder prepared in Example 6 after high temperature treatment are slightly worse than those in Example 1. The metallographic image of the solder obtained in Example 7 after high temperature treatment is tested, and the results are similar to those in Example 6.

[0108] The solders obtained in Examples 6 and 7 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Example 6 was 33.7 MPa, the Young's modulus was 16.6 MPa, and the tensile strength was 45.9 MPa. The yield strength obtained by the tensile test of the solder prepared in Example 7 was 33.2 MPa, the Young's modulus was 17.0 MPa, and the tensile strength was 46.3 MPa, indicating that the solders prepared in Examples 6-7 have good mechanical properties.

[0109] By comparing Example 1 with Examples 6-7, it can be seen that when the amount of cerium added is not within the most preferred range of the present application, the ability to inhibit the growth of IMC and inhibit further growth of IMC is slightly poor, and it will affect the further improvement of mechanical properties.

[0110] [Example 8]

[0111] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 41.57% by weight of tin, 1.3% by weight of zinc and 0.13% by weight of the rare earth element lanthanum, wherein the mass ratio of zinc to lanthanum is 10:1.

[0112] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0113] 14% bismuth, 43% lead and 41.57% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.3% zinc and 0.13% rare earth element (lanthanum) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0114] By performing the same morphology test on Example 8 as that on Example 1, a fine alloy structure can also be formed.

[0115] Fig.10 This is the metallographic image of the solder obtained in Example 8 after high-temperature treatment. It is found that the IMC size and thickness of the intermetallic compound of the low-temperature solder prepared in Example 8 are relatively low after high-temperature treatment, indicating that the formation and further growth of IMC can be effectively inhibited through the combined action of specific contents of zinc and lanthanum.

[0116] The solder obtained in Example 8 was subjected to a tensile test. The yield strength of the solder prepared in Example 8 obtained by the tensile test was 36 MPa, the Young's modulus was 18.8 MPa, and the tensile strength was 51.8 MPa, indicating that the solder prepared in Example 8 has good mechanical properties.

[0117] [Example 9]

[0118] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 42.15% by weight of tin, 0.75% by weight of zinc and 0.1% by weight of the rare earth element lanthanum, wherein the mass ratio of zinc to lanthanum is 7.5:1.

[0119] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0120] 14% bismuth, 43% lead and 42.15% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 0.75% zinc and 0.1% rare earth element (lanthanum) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0121] [Example 10]

[0122] The present embodiment provides a low-temperature solder, comprising 14% by weight of bismuth, 43% by weight of lead, 42.1% by weight of tin, 0.8% by weight of zinc and 0.1% by weight of the rare earth element lanthanum, wherein the mass ratio of zinc to lanthanum is 8:1.

[0123] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0124] 14% bismuth, 43% lead and 42.1% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 0.8% zinc and 0.1% rare earth element (lanthanum) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0125] By performing the same morphology test on Example 9 and Example 10 as that on Example 8, the test results are similar, and they also have fine alloy structures.

[0126] The solders obtained in Examples 9 and 10 were subjected to metallographic testing after high temperature treatment, and it was found that the IMC size and growth range of the intermetallic compounds of the low-temperature solders in Examples 9 and 10 after high temperature treatment were similar to those in Example 8.

[0127] The solders obtained in Examples 9 and 10 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Example 9 was 36.4 MPa, the Young's modulus was 18.2 MPa, and the tensile strength was 51.4 MPa. The yield strength obtained by the tensile test of the solder prepared in Example 10 was 35.9 MPa, the Young's modulus was 18.3 MPa, and the tensile strength was 52.2 MPa, indicating that the solders prepared in Examples 9-10 have good mechanical properties.

[0128] [Example 11]

[0129] The present embodiment provides a low-temperature solder, comprising 14% by mass of bismuth, 43% by mass of lead, 41.55% by mass of tin, 1.5% by mass of zinc and 0.15% by mass of the rare earth element neodymium, wherein the mass ratio of zinc to lanthanum is 10:1.

[0130] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0131] 14% bismuth, 43% lead and 41.55% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.3% zinc and 0.15% rare earth element (lanthanum) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0132] By performing the same morphology test on Example 11 as that on Example 1, a fine alloy structure can also be formed.

[0133] Fig.11 This is the metallographic diagram of the solder obtained in Example 11 after high-temperature treatment. It is found that the IMC size and thickness of the intermetallic compound of the low-temperature solder prepared in Example 11 are relatively low after high-temperature treatment, indicating that the formation and further growth of IMC can be effectively inhibited through the combined action of specific contents of zinc and neodymium.

[0134] The solder obtained in Example 11 was subjected to a tensile test. The yield strength of the solder prepared in Example 11 obtained by the tensile test was 35.6 MPa, the Young's modulus was 17.7 MPa, and the tensile strength was 53.4 MPa, indicating that the solder prepared in Example 11 has good mechanical properties.

[0135] [Example 12]

[0136] The present embodiment provides a low-temperature solder, comprising 14% by mass of bismuth, 43% by mass of lead, 41.93% by mass of tin, 1.04% by mass of zinc and 0.13% by mass of the rare earth element neodymium, wherein the mass ratio of zinc to lanthanum is 8:1.

[0137] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0138] 14% bismuth, 43% lead and 41.93% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.04% zinc and 0.13% rare earth element (lanthanum) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0139] [Example 13]

[0140] The present embodiment provides a low-temperature solder, including 14% by mass of bismuth, 43% by mass of lead, 41.64% by mass of tin, 1.2% by mass of zinc and 0.16% by mass of the rare earth element neodymium, wherein the mass ratio of zinc to lanthanum is 7.5:1.

[0141] This embodiment also provides a method for preparing a low-temperature solder, comprising:

[0142] 14% bismuth, 43% lead and 41.64% tin by weight are added to an alumina ceramic crucible, melted at 450°C and stirred for 30 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, and then 1.2% zinc and 0.16% rare earth element (lanthanum) are added, melted at 450°C and stirred for 60 minutes under the protection of a eutectic salt of potassium chloride and lithium chloride in a mass ratio of 1.3:1, the eutectic salt on the surface of the molten solder is scraped off, and the solder is cold-cast in a mold to form a low-temperature solder.

[0143] By performing the same morphology test on Example 12 and Example 13 as Example 11, the test results are similar, and they also have fine alloy structures.

[0144] The solders obtained in Example 12 and Example 13 were subjected to metallographic testing after high temperature treatment, and it was found that the IMC size and growth range of the intermetallic compounds of the low-temperature solders in Example 12 and Example 13 after high temperature treatment were similar to those in Example 11.

[0145] The solders obtained in Examples 12 and 13 were subjected to a tensile test. The yield strength obtained by the tensile test of the solder prepared in Example 12 was 35.7 MPa, the Young's modulus was 17.9 MPa, and the tensile strength was 54.2 MPa. The yield strength obtained by the tensile test of the solder prepared in Example 3 was 35.4 MPa, the Young's modulus was 17.5 MPa, and the tensile strength was 53.6 MPa, indicating that the solders prepared in Examples 12-13 have good mechanical properties.

[0146] The embodiment of the present application provides a photovoltaic module (not shown), including a solar cell and a welding ribbon. When the solar cell is a heterojunction solar cell, the commonly used welding ribbon is a low-temperature welding ribbon. The heterojunction solar cell and the low-temperature welding ribbon are directly welded together by the above-mentioned solder. Especially for heterojunction photovoltaic cells, the low-temperature welding ribbon is usually used for string welding.

[0147] Based on the matrix structure of the low-temperature solder strip, the use of the above-mentioned specific low-temperature solder can not only inhibit the growth of IMC in high-temperature environments such as subsequent component lamination and hot spots, maintain the stability of components in long-term use, but also effectively improve the mechanical properties, which is beneficial to the improvement of the tensile value after photovoltaic cell string welding.

[0148] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in the above embodiment. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid and then connected to the mains network to realize solar power supply.

[0149] It should be noted that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.

[0150] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0151] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.

[0152] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0153] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A low temperature solder, characterized in that: Taking the total mass of the low-temperature solder as 100%, the low-temperature solder comprises 14-26% by mass of bismuth, 37-43% by mass of lead, 0.1-1.5% by mass of zinc, 0.05-0.2% by mass of rare earth elements and the balance of tin.

2. The low temperature solder according to claim 1, characterized in that The ratio of the added amount of zinc to the rare earth element is (7.5-10):

1.

3. The low temperature solder according to claim 1, characterized in that The rare earth element includes any one of cerium, lanthanum, or neodymium, or a combination of at least two of them.

4. The low temperature solder according to claim 3, characterized in that When the rare earth element is cerium, the added amount of cerium is 0.08-0.12%.

5. The low temperature solder according to claim 3, characterized in that When the rare earth element is lanthanum, the added amount of lanthanum is 0.1-0.15%.

6. The low temperature solder according to claim 3, characterized in that When the rare earth element is neodymium, the added amount of neodymium is 0.13-0.16%.

7. A method for preparing a low-temperature solder according to any one of claims 1 to 6, characterized in that: The preparation method of the low temperature solder comprises: Bismuth with a mass percentage of 14-26%, lead with a mass percentage of 37-43% and the balance of tin are melt-mixed at 400-500° C. for 30-60 minutes, and then zinc with a mass percentage of 0.1-1.5% and rare earth elements with a mass percentage of 0.05-0.2% are added and melt-mixed for a second time at 400-500° C. for 60-120 minutes to obtain the low-temperature solder.

8. The preparation method according to claim 7, characterized in that: In the preparation process of the low-temperature solder, potassium chloride and lithium chloride eutectic salt with a mass ratio of (1-1.5):1 is used to cover the solder surface for protection; After the secondary melt mixing is uniform, the eutectic salt on the surface of the molten mixture is removed.

9. The preparation method according to claim 7, characterized in that: The preparation method further comprises: After the secondary melt mixing, cold casting is performed.

10. Use of the low-temperature solder according to any one of claims 1 to 5 in photovoltaic module processing.

Citation Information

Cited By

  • Low-temperature solder for photovoltaic solder strip of HJT heterojunction and preparation method of low-temperature solder

    CN119188022A

  • Method for improving cycling stability of negative electrode of aqueous zinc battery through ultrasonic vibration pressure