Laminated diamond-graphite copper-based composite material and preparation method thereof
By introducing diamond thermally conductive particles and chromium carbide connecting layers into the graphite/copper composite material, a three-dimensional thermal conductivity network is established, which solves the problems of low longitudinal thermal conductivity and difficult thickness control in the existing technology, and achieves efficient thermal management performance improvement.
Patent Information
- Application Number
- CN202410930782.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
Existing graphite/copper composite materials have low thermal conductivity in the longitudinal direction, making it difficult to meet the efficient heat dissipation requirements of electronic equipment, and the thickness of the composite material is difficult to control.
Diamond thermally conductive particles and graphite layers are alternately stacked and sintered through a porous copper template method to form a chromium carbide connection layer, establish a three-dimensional thermal conductivity network, improve the longitudinal thermal conductivity, and achieve one-step forming through vacuum hot pressing sintering.
It significantly improves the longitudinal thermal conductivity and thermal management performance of composite materials, enables controllable thermal conduction channels in the thickness direction, and enhances heat dissipation efficiency and material densification.
Smart Images

Figure CN118721885A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of metal-based composite materials and thermal management, and in particular to a laminated diamond-graphite copper-based composite material with a heat-conducting connection configuration and a preparation method thereof. Technical Background
[0002] As electronic devices become smaller and more powerful, the power density of electronic components continues to increase, and the heat generated also increases. High-performance computers, communication equipment, LED lighting, power electronics, and other fields are in urgent need of heat dissipation materials with excellent performance in order to effectively reduce the operating temperature of electronic components and improve the reliability and life of the equipment. Graphite / copper composites have attracted widespread attention due to their high thermal conductivity.
[0003] The thermal conductivity of graphite film with high thermal conductivity in the horizontal direction is as high as 2000W / (m﹒k), and the thermal conductivity in the longitudinal direction is less than one percent of that in the horizontal direction. After the graphite film is laminated with copper, it shows good thermal conductivity in the horizontal direction. The article "Fabrication of graphite films / copper composites by vacuum hot pressing for high-efficiency thermal management property" uses vacuum hot pressing to prepare laminated graphite film / copper composite materials, and its horizontal thermal conductivity is 485.2W / (m﹒k). Limited by the anisotropy of graphite film, the thermal conductivity of the composite material in the longitudinal direction is low. For example, Chinese patent CN103864067B prepares an ultra-high thermal conductivity graphite film / copper composite material, and its longitudinal thermal conductivity is only 60W / (m﹒k). Due to the addition of graphite, the longitudinal thermal conductivity of the composite material is obviously too low. On the other hand, with the increase in the number of graphite layers, the longitudinal thermal conductivity of the composite material decreases significantly. In many electronic devices, the required thickness of the heat dissipation material is 1-4mm. This often requires stacking dozens of graphite films. Since the longitudinal thermal conductivity of graphite is only about 10W / (m﹒k), graphite in the longitudinal direction is more like a thermal barrier layer rather than a thermal conductive layer.
[0004] One idea to solve the poor longitudinal thermal conductivity of stacked graphite film / copper composite materials is to use a high thermal conductivity phase to link the stacked graphite layers to each other, to open up the isolated graphite heat dissipation planes longitudinally, and to form a three-dimensional transmission heat conduction network. There are two key issues to be resolved: First, the high thermal conductivity phase and graphite need to be in close contact to ensure that the interface thermal resistance is as low as possible, which is the prerequisite for forming a three-dimensional thermal conduction network. Second, the configuration distribution of the high thermal conductivity phase needs to be controllably adjusted. In order to address the prominent problem of local hot spot heat dissipation in electronic components, more longitudinal heat conduction channels are configured at the hot spot position, so that the heat can be dissipated horizontally and efficiently transmitted longitudinally to each graphite layer, maximizing the heat dissipation effect of each graphite layer.
[0005] In view of the above problems, the present invention connects the upper and lower graphite layers by adding diamond thermal conductive particles, and uses a porous copper template method for sintering preparation. The designed porous copper template can accurately control the distribution configuration of diamond, and maximize its thermal performance in different scenarios; during the sintering process of the diamond-graphite / copper composite material, a chemical reaction occurs at the interface of the diamond-graphite film to form chromium carbide, making the interface connection tighter and connecting the vertical heat flow channel, thereby improving the longitudinal thermal conductivity; at the same time, the preparation method of the present invention can make the laminated diamond-graphite / copper composite material formed in one step, solving the problem that the thickness of the thermal management material is difficult to control. Summary of the invention
[0006] In order to overcome the defects in the prior art, the present invention provides a laminated diamond-graphite copper-based composite material with a heat-conducting connection configuration and a preparation method thereof, wherein the metal chromium layer plated on the surface of the diamond forms chromium carbide connected to each graphite layer during sintering, forming a three-dimensional heat-conducting network channel, thereby improving the thermal conductivity of the composite material in the longitudinal direction and realizing the controllable preparation of the heat-conducting channel in the thickness direction of the composite material.
[0007] To achieve the above object, the present invention adopts the following technical scheme: a laminated diamond-graphite copper-based composite material, wherein the laminated layer is a graphite-diamond alternating laminated structure, the composite material structure is a copper-filled alternating laminated structure, chromium carbide is used as a connecting layer between the graphite-diamond layers, the upper and lower layers are flaky graphite layers, the middle layer is a copper layer embedded with diamond particles, the two ends of the diamond are higher than the copper layer and penetrate into the graphite layer, and there is a chromium carbide layer at the contact interface between the graphite and the diamond.
[0008] The method for preparing the laminated diamond-graphite copper-based composite material comprises the following steps:
[0009] (1) coating diamond particles with a chromium layer;
[0010] (2) forming a preform by using diamond, graphite film and porous copper template;
[0011] (3) The preform is subjected to vacuum hot pressing and sintering to prepare a laminated diamond-graphite copper-based composite material.
[0012] Preferably, in the method for preparing the laminated diamond-graphite copper-based composite material, the diamond in step (1) is artificially synthesized single crystal particles with a particle size of 300 μm and a volume fraction of 30%.
[0013] Preferably, the graphite film in step (1) has a thickness of 70 μm and a density of 2.1 g / cm 3 .
[0014] Preferably, the porous copper template is a copper-chromium alloy substrate with a chromium content of 0.2 wt %, a pore size of 300 μm and a thickness of 320 μm.
[0015] Preferably, the thickness of the chromium layer plated on the diamond surface in step (1) is 100 nm.
[0016] Preferably, the specific process of forming the preform of the diamond, graphite film and porous copper template in step (2) is as follows: diamond particles are evenly dispersed in the holes of the porous copper template, and the porous copper template containing diamond and the graphite film are stacked and placed alternately to finally form a composite material with a total thickness of 0.5-10 mm.
[0017] Preferably, the porous copper templates are stacked so that the diamond particles are arranged in a straight line in the vertical direction in order to achieve the best heat dissipation effect in the longitudinal direction (ie, the vertical direction).
[0018] Preferably, the vacuum hot pressing sintering in step (3) is specifically to heat the preform to 600°C at a heating rate of 20°C / min in a vacuum below 10Pa, keep the temperature for 10min, continue to heat to 950°C at the same heating rate, apply a pressure of 15MPa, keep the pressure and keep the temperature for 60min, so that the diamond penetrates 15μm into the graphite layer and reacts with the chromium layer to form chromium carbide, and cool to obtain a laminated diamond / chromium carbide / graphite copper-based composite material, wherein the thickness of the laminated composite material is 0.5-10mm.
[0019] Therefore, the beneficial effects of the present invention are: a chromium layer is plated on the diamond, and the diamond is dispersed in the holes of the customized porous copper template. The porous copper template can be designed with different hole distribution configurations according to different application scenarios. The holes have a positioning effect on the diamond, effectively avoiding the agglomeration of the diamond. The porous copper template for placing the diamond is placed alternately with the graphite film, and a special structure preform with one-to-one correspondence between the points of each layer of diamond is formed. Through vacuum hot pressing sintering, the diamond penetrates the graphite layer and reacts with the chromium layer to form chromium carbide, and the laminated diamond / chromium carbide / graphite chemically connected copper-based composite material is obtained by cooling. The present invention plates a chromium layer on the diamond, and forms a preform with the diamond, graphite film and porous copper template coated with the chromium layer by physical vapor deposition for hot pressing sintering. The chromium metal layer begins to generate chromium carbide with graphite at 700°C, and generates Cr7C3 and Cr3C2 at 900-950°C. After sintering, a laminated diamond-chromium carbide-graphite high thermal conductivity bridge is obtained. The bonding strength between the copper matrix and the diamond reinforcement is greatly improved, and the thermal conductivity of the composite material is improved. The benefits of diamond and graphite as heat conduction channels. The chemical connection of the interface is achieved. The resulting diamond-chromium carbide-graphite interface avoids contact with the copper matrix, and the interface is pure and has low thermal resistance. Using the copper template sintering method, the arrangement of diamonds can be designed and changed according to the different directions of heat flow to achieve the highest utilization efficiency. This method is simple and efficient, and combines the heat treatment of the interface connection and the densification sintering steps of the composite material to achieve the gradient preparation of the heat conduction channel in the thickness direction.
[0020] The present invention can design different mesh configurations on copper foil by laser or mechanical drilling, etc., diamonds are filled in the designed holes as longitudinal heat conduction channels, and a laminated diamond-graphite copper-based composite material with high transverse and longitudinal thermal conductivity and certain mechanical strength is prepared by vacuum hot pressing and sintering. The thickness of the composite material can be adjusted by the number of layers, the preparation process is simple, and the application scenarios are wide. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the structure of the seven-layered diamond-graphite copper-based composite material according to Example 1 and Example 2 of the present invention and a schematic diagram of the method of contact between graphite and diamond.
[0022] Figure 2 It is a schematic diagram of a porous copper template with a volume fraction of 30% and uniform distribution using laser drilling in an embodiment of the present invention.
[0023] Figure 3 It is a schematic diagram of a non-uniform configuration of designing a high volume fraction of diamond heat dissipation in a heat source concentrated area in Example 8 of the present invention.
[0024] Figure 4It is a schematic diagram of a stepped diamond configuration design for a heat source and a heat dissipation system that are not on the same horizontal line in Example 9 of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1:
[0027] Diamond with a particle size of 300 μm and a volume fraction of 30% was selected for vacuum evaporation chromium plating. Figure 2 Schematic diagram of a porous copper template with a volume fraction of 30% uniformly distributed by laser drilling in an embodiment of the present invention, and the vacuum degree is maintained at 10 - 3 Pa, diamond and chromium powder with a particle size of 1 μm are evenly mixed, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is 8, and the number of porous copper templates is 7. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based composite material with a horizontal thermal conductivity of 796W / (m﹒k) and a longitudinal thermal conductivity of 252W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm. Figure 1 It is a schematic diagram of the structure of the seven-layered diamond-graphite copper-based composite material in Example 1 of the present invention and a schematic diagram of the method of contact between graphite and diamond.
[0028] Embodiment 2:
[0029] Diamond with a particle size of 300 μm and a volume fraction of 30% was selected for vacuum evaporation chromium plating. Figure 2 Schematic diagram of a porous copper template with a volume fraction of 30% uniformly distributed by laser drilling in an embodiment of the present invention, and the vacuum degree is maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are evenly mixed, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is 18, and the number of porous copper templates is 17. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based composite material with a horizontal thermal conductivity of 681W / (m﹒k) and a longitudinal thermal conductivity of 189W / (m﹒k) is obtained. The total thickness of the composite material is 5.2mm.
[0030] Embodiment 3:
[0031] Diamond with a particle size of 300 μm and a volume fraction of 30% was selected for vacuum evaporation chromium plating. Figure 2 Schematic diagram of a porous copper template with a volume fraction of 30% uniformly distributed by laser drilling in an embodiment of the present invention, and the vacuum degree is maintained at 10 - 3 Pa, diamond and chromium powder with a particle size of 1 μm are evenly mixed, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is 28, and the number of porous copper templates is 27. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based 27-layer composite material with a horizontal thermal conductivity of 568W / (m﹒k) and a longitudinal thermal conductivity of 156W / (m﹒k) is obtained. The total thickness of the composite material is 8.2mm.
[0032] Embodiment 4:
[0033] Diamond with a particle size of 300 μm and a volume fraction of 20% was selected for vacuum evaporation chromium plating, and the vacuum degree was maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are evenly mixed, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer. The graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 723W / (m﹒k) and a longitudinal thermal conductivity of 220W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm. The composite material is bonded to the chip and placed on a 50℃ constant temperature heat source. A cooling system is placed on the other side of the composite material to simulate the working state of the chip. After 15s, the temperature of the chip surface is measured to be 36.5℃.
[0034] Embodiment 5:
[0035] Diamond with a particle size of 300 μm and a volume fraction of 10% was selected for vacuum evaporation chromium plating, and the vacuum degree was maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are mixed evenly, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued to 10-3Pa. After cooling to room temperature, a chromium-coated diamond with a coating thickness of 100nm is obtained. The thickness of 70μm and the density of 2.1g / cm 3Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 640W / (m﹒k) and a longitudinal thermal conductivity of 170W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm.
[0036] Embodiment 6:
[0037] Diamond with a particle size of 300 μm and a volume fraction of 40% was selected for vacuum evaporation chromium plating. The vacuum degree was maintained at 10-3 Pa. Diamond and chromium powder with a particle size of 1 μm were mixed evenly. The coating temperature was 800 °C and the coating time was 2 h. During the heating stage, chromium vapor was deposited on the surface of the diamond. After the deposition was completed, the residual gas was extracted and the vacuum was continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 1000℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 30min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 786W / (m﹒k) and a longitudinal thermal conductivity of 223W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm.
[0038] Embodiment 7:
[0039] Diamond with a particle size of 300 μm and a volume fraction of 30% was selected for vacuum evaporation chromium plating, and the vacuum degree was maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are mixed evenly, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued to 10-3Pa. After cooling to room temperature, a chromium-coated diamond with a coating thickness of 100nm is obtained. The thickness of 30μm and the density of 2.1g / cm 3Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 10MPa is applied at the same time. The pressure is kept for 30min, so that the diamond penetrates the graphite layer by 10μm, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 828W / (m﹒k) and a longitudinal thermal conductivity of 276W / (m﹒k) is obtained. The total thickness of the composite material is 1.7mm.
[0040] Embodiment 8:
[0041] Diamond with a particle size of 300 μm and a volume fraction of 30% was selected for vacuum evaporation chromium plating, and the vacuum degree was maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are mixed evenly, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued to 10-3Pa. After cooling to room temperature, a chromium-coated diamond with a coating thickness of 100nm is obtained. The thickness of 70μm and the density of 2.1g / cm 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, graphite and porous copper templates are alternately stacked, the total number of graphite layers is eight, and the porous copper template is seven. The stacked blank is placed in a vacuum below 10Pa, heated to 600℃ at a heating rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 20MPa is applied at the same time (the problem is the same as in Example 5). The pressure is maintained for 30min, so that the diamond penetrates 20μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 709W / (m﹒k) and a longitudinal thermal conductivity of 213W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm.
[0042] Embodiment 9:
[0043] Diamond with a particle size of 500 μm and a volume fraction of 30% was selected for vacuum evaporation chromium plating, and the vacuum degree was maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are mixed evenly, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued to 10-3Pa. After cooling to room temperature, a chromium-coated diamond with a coating thickness of 100nm is obtained. The thickness of 70μm and the density of 2.1g / cm 3Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 30MPa is applied at the same time. The pressure is kept for 30min, so that the diamond penetrates 30μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 703W / (m﹒k) and a longitudinal thermal conductivity of 221W / (m﹒k) is obtained. The total thickness of the composite material is 3.6mm.
[0044] Embodiment 10:
[0045] Diamond with a particle size of 300 μm, a volume fraction of 30% in the middle half of the area, and 10% in the remaining half of the area was selected for vacuum evaporation chromium plating. Figure 3 Schematic diagram of a non-uniform configuration of a heat source concentrated area designed with a high volume fraction of diamond heat dissipation in an embodiment of the present invention, and the vacuum degree is maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are evenly mixed, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 746W / (m﹒k) and a longitudinal thermal conductivity of 237W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm. The composite material was bonded to the chip and placed on a constant temperature heat source of 50°C. A cooling system was placed on the other side of the composite material to simulate the working state of the chip. After 15 seconds, the temperature of the chip surface was measured to be 35°C, which was 1.5°C lower than that of Example 2 with the same diamond volume fraction, indicating that the composite material of this configuration has higher heat dissipation efficiency.
[0046] Embodiment 11:
[0047] Diamond with a particle size of 300 μm, a volume fraction of 30% in the half-step area, and 10% in the other areas was selected for vacuum evaporation chromium plating. Figure 4 This is a schematic diagram of a stepped diamond configuration design for a heat source and a heat dissipation system that are not on the same horizontal line. The vacuum degree is maintained at 10 -3 Pa, diamond and chromium powder with a particle size of 1 μm are evenly mixed, the coating temperature is 800℃, the coating time is 2h, and chromium vapor is deposited on the diamond surface during the heating stage. After the deposition is completed, the residual gas is extracted and the vacuum is continued for 10 -3 Pa, cooled to room temperature, and a chromium-coated diamond with a coating thickness of 100 nm was obtained. 3 Graphite sheets. Diamonds are evenly distributed in the porous copper template, graphite sheets are stacked, and graphite and porous copper templates are alternately stacked. The total number of graphite layers is eight, and the number of porous copper templates is seven. The stacked body is placed in a vacuum below 10Pa, heated to 600℃ at a rate of 20℃ / min, and kept warm for 10min. At the same heating rate, the temperature is continued to rise to 950℃, and a pressure of 15MPa is applied at the same time. The pressure is kept for 60min, so that the diamond penetrates 15μm into the graphite layer, and the graphite reacts with the chromium layer to form chromium carbide. After cooling, a diamond / chromium carbide / graphite copper-based laminated composite material with a horizontal thermal conductivity of 705W / (m﹒k) and a longitudinal thermal conductivity of 211W / (m﹒k) is obtained. The total thickness of the composite material is 2.2mm. The composite material was bonded to the chip and placed on a constant temperature heat source of 50°C. A cooling system was placed on the other side of the composite material to simulate the working state of the chip. After 15 seconds, the temperature of the chip surface was measured to be 35.3°C, which was 1.2°C lower than that of Example 2 with the same diamond volume fraction, indicating that the composite material of this configuration has higher heat dissipation efficiency.
[0048] The above-described embodiment is only a preferred solution of the present invention and does not limit the invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.
Claims
1. A laminated diamond-graphite copper-based composite material, It is characterized in that The stacked layers are graphite-diamond alternating stacked structures, the composite material structure is copper-filled alternating stacked structures, chromium carbide is used as a connecting layer between the graphite-diamond layers, the upper and lower layers are flaky graphite layers, the middle layer is a copper layer embedded with diamond particles, the two ends of the diamond are higher than the copper layer and penetrate into the graphite layer, and there is a chromium carbide layer at the contact interface between the graphite and the diamond.
2. The method for preparing the laminated diamond-graphite copper-based composite material according to claim 1, It is characterized in that The steps include: (1) coating diamond particles with a chromium layer; (2) forming a preform by using diamond, graphite film and porous copper template; (3) The preform is subjected to vacuum hot pressing and sintering to prepare a laminated diamond-graphite copper-based composite material.
3. The method for preparing the laminated diamond-graphite copper-based composite material according to claim 2, It is characterized in that The diamond in step (1) is an artificially synthesized single crystal particle with a particle size of 100-500 μm and a density of 3.47-3.56 g / cm 3 , volume fraction is 10-30%.
4. The method for preparing the laminated diamond-graphite copper-based composite material according to claim 2, It is characterized in that The graphite film in step (1) has a thickness of 30-100 μm and a density of 1.7-2.3 g / cm 3 .
5. The method for preparing the laminated diamond-graphite copper-based composite material as claimed in claim 2, It is characterized in that The porous copper template is a copper-chromium alloy substrate with a chromium content of 0.1-5wt%, a pore size of 110-510 μm, and a thickness of 100-520 μm.
6. The method for preparing the laminated diamond-graphite copper-based composite material according to claim 2, It is characterized in that The thickness of the chromium layer plated on the diamond surface in step (1) is 10-110 nm.
7. The method for preparing the laminated diamond-graphite copper-based composite material as claimed in claim 2, It is characterized in that The specific process of forming a preform from diamond, graphite film and porous copper template in step (2) is as follows: diamond particles are evenly dispersed in the holes of the porous copper template, the porous copper template containing diamond and the graphite film are stacked and placed alternately, and finally a composite material with a total thickness of more than 0.2 mm is formed.
8. The method for preparing the laminated diamond-graphite copper-based composite material according to claim 7, It is characterized in that The porous copper templates are stacked so that the diamond particles are aligned in the vertical direction.
9. The method for preparing the laminated diamond-graphite copper-based composite material as claimed in claim 2, It is characterized in that The vacuum hot pressing sintering in step (3) is specifically to heat the preform to 600°C at a heating rate of 20°C / min in a vacuum below 10Pa, keep the temperature for 10min, continue to heat to 850-1000°C at the same heating rate, apply a pressure of 10-30MPa at the same time, keep the pressure and keep the temperature for 30-60min, so that the diamond penetrates the graphite layer by 10-30μm and reacts with the chromium layer to form chromium carbide, and cool to obtain a laminated diamond / chromium carbide / graphite copper-based composite material, wherein the laminated composite material has a thickness of 0.5-5mm.
Citation Information
Patent Citations
Diamond / copper high-thermal conductivity composite material and preparation method thereof
CN102108458A
Micro-through-hole Cu-based CVD diamond heat sink sheet and preparation method thereof
CN110690186A
Preparation method of high-thermal-conductivity and low-expansion Diamond-Cu composite material with sandwich structure
CN111455205A
Heat sink, its manufacture method and package using the same
JP1997312362A
Cited By
Vacuum sintering material, preparation method thereof, vacuum sintering device and application of vacuum sintering device
CN121226030A