Laminated film and method for producing laminated film
By using an anti-adhesive agent with a particle size of less than 1.3 μm and an appropriate amount of resin composition in the laminated film, an excellent base film and adhesive layer are formed, which solves the problems of misdetection and adhesion during pasting and realizes the control of the adherend. for precise inspection and efficient stripping.
Patent Information
- Application Number
- CN202410253097.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-01
AI Technical Summary
When the existing laminated film is pasted to the adherend, it is easy to cause misdetection due to the anti-adhesive agent, which affects the accuracy of the optical inspection. It is also easy to stick during winding, making recycling difficult.
A combination of a base film and an adhesive layer is used. The base film contains an anti-adhesive agent of less than 1.3 μm. The anti-adhesive agent content is in the range of 350 ppm to 3000 ppm. The resin composition is formed after filtering through a screen to prepare the base film. And an adhesive layer is formed on it to ensure anti-adhesion and optical properties.
It achieves precise optical inspection of the adherend in the pasted state, reduces the risk of adhesion during pasting, and ensures the excellent anti-adhesion and efficient peeling performance of the laminated film.
Smart Images

Figure CN118721900A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated film and a method for producing the laminated film. Background Art
[0002] It is known that a laminated film having a substrate film and an adhesive layer is pasted on the surface of various industrial products for various purposes. As the purpose of pasting the laminated film, the surface of the adherend can be protected, etc. As such a laminated film, for example, a surface protective film for polarizer having a support film and an adhesive layer formed on one side of the support film is proposed (reference patent document 1).
[0003] After pasting a release liner on the surface of the adhesive layer on the opposite side of the substrate film, such a laminated film is sometimes rolled up into a roll for recovery. However, when the laminated film including the release liner is rolled up into a roll, there is a possibility that the substrate film and the release liner will stick together.
[0004] Therefore, research has been conducted to include an anti-adhesion agent (hereinafter referred to as an AB agent) on the base film to inhibit the adhesion between the base film and the release liner. However, in recent years, when the laminated film is sometimes adhered to the adherend and an optical inspection is performed after the laminated film containing the AB agent is adhered to the adherend, false detection may occur due to the AB agent, and the adherend may not be correctly inspected.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2017-32768 Summary of the invention
[0008] Problems to be solved by the invention
[0009] The present invention is made to solve the above-mentioned previous problems, and its main purpose is to provide a laminated film and a method for manufacturing the same, wherein the laminated film has excellent anti-adhesion properties and can inspect the adherend with good accuracy even when the laminated film is provided for optical inspection in the state of being adhered to the adherend.
[0010] Means for solving problems
[0011] [1] According to one embodiment, a laminated film comprises a substrate film and an adhesive layer. The adhesive layer is laminated on the substrate film. The substrate film comprises a resin material as a matrix and an anti-blocking agent dispersed in the resin material. The average primary particle size of the anti-blocking agent is 1.3 μm or less. The content ratio of the anti-blocking agent in the substrate film is 350 ppm to 3000 ppm.
[0012] [2] In the laminated film described in [1], the base film has a unit area of 10 cm 2 The number of defects having a maximum Feret diameter of 30 μm or more may be 5 or less.
[0013] [3] In the laminated film described in [1] or [2] above, the in-plane retardation Re (550) of the substrate film may be 10 nm or less.
[0014] [4] In the laminated film according to any one of [1] to [3] above, the dynamic friction coefficient of the substrate film may be 1.0 or less.
[0015] [5] The peeling force of the laminated film according to any one of [1] to [4] above may be 3.0 N / 25 mm or less at a tensile speed of 30 m / min and a peeling angle of 180°.
[0016] [6] In the laminated film described in any one of [1] to [5] above, the resin material may include a polycarbonate-based resin and / or a cycloolefin-based resin.
[0017] [7] According to another aspect of the present invention, a method for manufacturing a laminated film comprises: a step of preparing a resin composition by mixing a molten resin material with an anti-blocking agent; a step of passing the resin composition through a filter; a step of preparing a substrate film by extruding the resin composition after passing through the filter; and a step of forming an adhesive layer on the substrate film. The average primary particle size of the anti-blocking agent is 1.3 μm or less. The content ratio of the anti-blocking agent in the resin composition is 350 ppm to 3000 ppm.
[0018] [8] In the method for producing a laminated film according to [7], the filter may be a mesh having a mesh size of 0.035 mm to 0.070 mm.
[0019] Effects of the Invention
[0020] According to the embodiment of the present invention, it is possible to realize a laminate film having excellent anti-blocking properties, and even when the laminate film is subjected to optical inspection in a state of being attached to an adherend, the adherend can be inspected with high accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention.
[0022] Figure 2 is included Figure 1 A schematic cross-sectional view of an optical component with a laminated film.
[0023] Description of the Figure Symbols
[0024] 1. Substrate film
[0025] 2 Adhesive layer
[0026] 100 laminated film. DETAILED DESCRIPTION
[0027] Hereinafter, representative embodiments of the present invention will be described, but the present invention is not limited to these embodiments. In addition, in order to make the description clearer, the drawings sometimes schematically show the width, thickness, shape, etc. of each part compared with the embodiments, but this is only an example and does not limit the interpretation of the present invention.
[0028] (Definition of terms and symbols)
[0029] The definitions of terms and symbols in this specification are as follows.
[0030] (1) Refractive index (nx, ny, nz)
[0031] “nx” is the refractive index in the direction where the refractive index in the plane reaches the maximum (ie, the slow axis direction), “ny” is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and “nz” is the refractive index in the thickness direction.
[0032] (2) In-plane phase difference (Re)
[0033] "Re(λ)" is the in-plane phase difference measured by light of wavelength λnm at 23°C. For example, "Re(550)" is the in-plane phase difference measured by light of wavelength 550nm at 23°C. Re(λ) is obtained by the formula: Re(λ) = (nx-ny) × d when the thickness of the layer (film) is set to d (nm).
[0034] (3) Retardation in the thickness direction (Rth)
[0035] "Rth(λ)" is the phase difference in the thickness direction measured by light of wavelength λnm at 23°C. For example, "Rth(550)" is the phase difference in the thickness direction measured by light of wavelength 550nm at 23°C. Rth(λ) is obtained by the formula: Rth(λ) = (nx-nz) × d when the thickness of the layer (film) is set to d (nm).
[0036] A. Overall structure of laminated film
[0037] Figure 1 This is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention.
[0038] The laminated film 100 shown in the figure comprises a substrate film 1 and an adhesive layer 2. The adhesive layer 2 is laminated on the substrate film 1. The substrate film 1 comprises a resin material as a matrix and an anti-blocking agent (hereinafter referred to as AB agent) dispersed in the resin material. The AB agent is typically in a particle form, and is dispersed in the resin material as an aggregate formed by agglomeration of a plurality of AB agent particles. The average primary particle size of the AB agent is 1.3 μm or less. The content ratio of the AB agent in the substrate film 1 (based on mass) is 350 ppm to 3000 ppm.
[0039] If the content ratio of the AB agent is within such a range, the laminated film can be given excellent anti-adhesion properties. In addition, if the average primary particle size of the AB agent is within such a range, even when the laminated film is attached to an adherend and subjected to optical inspection, false detection caused by the AB agent (especially the agglomerates of the AB agent) can be suppressed, and as a result, the adherend can be inspected with good accuracy. In other words, the result of inspecting the adherend with the laminated film attached can be matched with the result of inspecting only the adherend.
[0040] The average primary particle size of the AB agent is preferably 1.0 μm or less. On the other hand, the lower limit of the average primary particle size of the AB agent is typically 0.1 μm or less. The average primary particle size of the AB agent can be measured by a laser diffraction method.
[0041] When the average primary particle size of the AB agent is within such a range, it is possible to stably suppress the occurrence of erroneous detection of the AB agent (particularly, agglomerates of the AB agent) in optical inspection of an adherend.
[0042] The content ratio (based on mass) of the AB agent in the base film 1 is preferably 500 ppm to 3000 ppm, and more preferably 500 ppm to 2000 ppm.
[0043] When the content ratio of the AB agent is within such a range, the anti-blocking property can be sufficiently imparted to the laminated film, and the AB agent (especially the agglomerates of the AB agent) can be more stably suppressed from being erroneously detected during optical inspection of the adherend.
[0044] The unit area of the substrate film 1 is 10 cm 2 The number of defects with a maximum Feret diameter of 30 μm or more (hereinafter referred to as D30 / 10 cm of the substrate film) 2 ) is, for example, 5 or less, preferably 3 or less. D30 / 10cm of the substrate film 2 The lower limit of is typically 0. In addition, the method for measuring the number of defects will be described in the examples described later.
[0045] D30 / 10cm of base film 2Within such a range, in optical inspection of an adherend, erroneous detection due to the base film can be suppressed, and as a result, the inspection accuracy of the adherend can be improved.
[0046] In addition, the unit area of the base film 1 is 10 cm 2 The number of defects with a maximum Feret diameter of less than 30 μm is not particularly limited. Unit area 10 cm 2 The number of defects with a maximum Feret diameter of less than 30 μm and not less than 10 μm is, for example, 15 or less, preferably 10 or less. Unit area 10 cm 2 The lower limit of the number of defects having a maximum Feret diameter of less than 30 μm and 10 μm or more is typically 0.
[0047] Examples of defects in the base film 1 include: aggregates of the AB agent; foreign matter such as fibers mixed in the resin material; gel-like matter generated by thermal crosslinking of the resin material; and bubbles generated by moisture in the resin.
[0048] The base film 1 is typically optically isotropic. In this specification, the term "optically isotropic" means that the in-plane retardation Re (550) and the thickness direction retardation Rth (550) are within the following ranges.
[0049] The in-plane retardation Re(550) of the base film 1 is, for example, 10 nm or less, preferably 5 nm or less, and more preferably 3 nm or less. On the other hand, the lower limit of the in-plane retardation Re(550) of the base film 1 is typically 0 nm.
[0050] When the in-plane retardation Re (550) of the base film is within such a range, rainbow spots (rainbow fringes) of the base film in optical inspection can be well suppressed, and as a result, the inspection accuracy of the adherend can be improved.
[0051] The retardation Rth(550) in the thickness direction of the base film 1 is in the range of, for example, -10 nm to +10 nm, or preferably -5 nm to +5 nm.
[0052] The dynamic friction coefficient of the base film 1 is, for example, 1.2 or less, and preferably 1.0 or less. On the other hand, the lower limit of the dynamic friction coefficient of the base film 1 is typically 0.2. The dynamic friction coefficient of the base film can be measured according to JIS K7125.
[0053] When the dynamic friction coefficient of the base film is within such a range, excellent anti-blocking properties can be stably imparted to the laminated film.
[0054] The peeling force of the laminated film 100 to the acrylic plate is, for example, 3.5 N / 25 mm or less, preferably 3.0 N / 25 mm or less, more preferably 2.5 N / 25 mm or less, and further preferably 2.0 N / 25 mm or less at a tensile speed of 30 m / min and a peeling angle of 180°. If the laminated film has such a peeling force, the laminated film can be smoothly peeled off from the adherend after optical inspection.
[0055] On the other hand, the peeling force of the laminated film 100 to the polyacrylate plate is, for example, 0.5 N / 25 mm or more, preferably 1.0 N / 25 mm or more, and preferably 1.2 N / 25 mm or more. If the laminated film has such a peeling force, the laminated film can stably follow the surface of the adherend when the laminated film is attached to the adherend. It should be noted that the above-mentioned peeling force can be measured according to JIS Z0237, and more specifically, can be measured by the following peeling force test.
[0056] (Peel force test)
[0057] The laminated film was cut into a rectangular shape of 25 mm × 100 mm to prepare a sample; the sample was roller-bonded to the surface of an acrylic plate through the adhesive layer at a pressure of 0.25 MPa and a conveying speed of 0.3 m / min; the sample attached to the acrylic plate was allowed to stand for 30 minutes at a temperature of 23°C and a relative humidity of 50%, and then peeled at a peeling angle of 180° and a tensile speed of 30 m / min under the same environment to measure the peeling force.
[0058] Hereinafter, components of the laminated film will be described.
[0059] B. Substrate film
[0060] The substrate film 1 includes a resin material as a main component. As specific examples of the resin material, cycloolefin (COP) systems such as polynorbornene systems; polyester systems such as polyethylene terephthalate (PET) systems; cellulose resins such as triacetyl cellulose (TAC); polycarbonate (PC) systems; (meth) acrylic acid systems; polyvinyl alcohol systems; polyamide systems; polyimide systems; polyether sulfone systems; polysulfone systems; polystyrene systems; polyolefin systems; transparent resins such as acetate systems. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid systems, urethane systems, (meth) acrylic urethane systems, epoxy systems, and siloxane systems can also be listed. It should be noted that "(meth) acrylic acid resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers can also be listed, for example. In addition, polymers described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the polymer, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group on the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group on the side chain can be used, for example, a resin composition containing an alternating copolymer made of isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The materials of the resin film can be used alone or in combination.
[0061] In one embodiment, the resin material of the base film 1 is amorphous. When the base film is made of an amorphous resin material, excellent transparency can be imparted to the laminated film.
[0062] Among these resin materials, preferably, PC-based resins and COP-based resins are used, and more preferably, PC-based resins are used.
[0063] In one embodiment, the PC-based resin contains at least a constituent unit derived from a dihydroxy compound having a bonding structure represented by the following structural formula (1), and is produced by reacting a dihydroxy compound with a carbonic acid diester in the presence of a polymerization catalyst, wherein the dihydroxy compound contains at least a constituent unit having at least one bonding structure -CH 2 In other words, the PC-based resin contains a structural unit derived from a dihydroxy compound and a carbonate group derived from a carbonic acid diester.
[0064]
[0065] Here, the dihydroxy compound having the bond structure represented by the structural formula (1) is any compound having two alcoholic hydroxyl groups and a linking group -CH 2Any compound having a -O- structure may be used as long as it can react with a carbonic acid diester in the presence of a polymerization catalyst to produce a polycarbonate, and a plurality of compounds may be used in combination.
[0066] In addition, as a dihydroxy compound for PC-based resins, a dihydroxy compound that does not have a bonding structure represented by the above-mentioned structural formula (1) may also be used in combination. Hereinafter, a dihydroxy compound having a bonding structure represented by the structural formula (1) is sometimes referred to as a dihydroxy compound (A), and a dihydroxy compound that does not have a bonding structure represented by the structural formula (1) is sometimes referred to as a dihydroxy compound (B).
[0067] (Dihydroxy compound (A))
[0068] The "linking group -CH 2 "-O-" means a structure in which atoms other than hydrogen atoms are bonded to each other to form a molecule. In the linking group, the atom that can be bonded to at least an oxygen atom or the atom that can be bonded to both a carbon atom and an oxygen atom is preferably a carbon atom. The "linking group -CH 2 The number of "-O-" is preferably 1 or more, more preferably 2 to 4.
[0069] Specific examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-di ...isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene Compounds having an aromatic group on the side chain and an ether group bonded to the aromatic group on the main chain, such as bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene; such as bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, 2,2 -bis[3,5-dimethyl-4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxyethoxy)-3-isopropylphenyl]propane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2- Bis(hydroxyalkoxyaryl)alkanes such as bis[4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane, and 2,2-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane; Bis(hydroxyalkoxyaryl)cycloalkanes such as 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane;Dihydroxyalkoxydiaryl ethers such as 4,4'-bis(2-hydroxyethoxy)diphenyl ether and 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxyaryl sulfides such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxyaryl sulfoxides such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfoxide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfoxide; -(2-dihydroxyethoxy)-3-methylphenyl] sulfone; bishydroxyalkoxybenzenes such as 1,4-bishydroxyethoxybenzene; 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene; 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene; 4,4'-bis(2-hydroxyethoxy)biphenyl; 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane; anhydrous sugar alcohols such as exemplified by the dihydroxy compound represented by the following formula (2); and compounds having a cyclic ether structure such as exemplified by the spiroglycol represented by the following general formula (3). The dihydroxy compound (A) may be used alone or in combination. ;
[0070]
[0071] Among these dihydroxy compounds (A), preferably, dihydroxy compounds represented by the above formula (2) can be cited. As dihydroxy compounds represented by the above formula (2), isosorbide, isomannide, and isoidide, which are in a stereoisomer relationship, can be cited. These can be used alone or in combination of two or more.
[0072] Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches that are abundant in resources and easily available is most preferred from the viewpoints of availability and ease of production, optical properties, and moldability.
[0073] The proportion of the structural units derived from the dihydroxy compound (A) relative to the structural units derived from all dihydroxy compounds contained in the PC-based resin is, for example, 10 mol% or more, preferably 40 mol% or more, and more preferably 60 mol% or more. On the other hand, the proportion of the structural units derived from the dihydroxy compound (A) is, for example, 100 mol% or less, preferably 90 mol% or less, more preferably 80 mol% or less, and further preferably 70 mol% or less. If the proportion of the dihydroxy compound (A) is within the above range, the rainbow spots of the substrate film in optical inspection can be stably suppressed.
[0074] (Dihydroxy compound (B))
[0075] As a dihydroxy compound forming a structural unit of the PC-based resin, a dihydroxy compound (B) may be used together with the dihydroxy compound (A). When the dihydroxy compounds (A) and (B) are used in combination, rainbow spots of the substrate film in optical inspection can be more stably suppressed.
[0076] The dihydroxy compound (B) is typically a dihydroxy compound other than the dihydroxy compound (A). Examples of the dihydroxy compound (B) include alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure. The dihydroxy compound (B) may be used alone or in combination.
[0077] Among the dihydroxy compounds (B), preferably, an alicyclic dihydroxy compound is used.
[0078] The alicyclic dihydroxy compound is not particularly limited, but preferably includes compounds generally containing a five-membered ring structure or a six-membered ring structure. In addition, the six-membered ring structure can be fixed to a chair shape or a boat shape by a covalent bond. When the alicyclic dihydroxy compound is a five-membered ring or a six-membered ring structure, the heat resistance of the obtained PC-based resin can be improved. The number of carbon atoms contained in the alicyclic dihydroxy compound is, for example, 70 or less, preferably 50 or less, and more preferably 30 or less.
[0079] Specific examples of the alicyclic dihydroxy compound containing a five-membered ring structure or a six-membered ring structure include alicyclic dihydroxy compounds represented by the following general formula (I) or (II).
[0080] HOCH 2 -R 1 -CH 2 OH (I)
[0081] HO-R 2 -OH (II)
[0082] (In formula (I) and (II), R1 and R 2 Each of them represents a cycloalkyl group having 4 to 20 carbon atoms. )
[0083] Cyclohexanedimethanol as the alicyclic dihydroxy compound represented by the general formula (I) includes R 1 By the following general formula (Ia) (wherein, R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. ) represents various isomers. Specific examples of such compounds include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.
[0084]
[0085] The tricyclodecane dimethanol or pentacyclopentadecanedimethanol as the alicyclic dihydroxy compound represented by the general formula (I) comprises R 1 Various isomers represented by the following general formula (Ib) (wherein n represents 0 or 1).
[0086]
[0087] The alicyclic dihydroxy compound represented by the general formula (I) is decalin dimethanol or tricyclotetradecane dimethanol, which includes R 1 Various isomers represented by the following general formula (Ic) (wherein m represents 0 or 1). Specific examples of such compounds include 2,6-decalinedimethanol, 1,5-decalinedimethanol, and 2,3-decalinedimethanol.
[0088]
[0089] The norbornane dimethanol as the alicyclic dihydroxy compound represented by the general formula (I) comprises R 1 Various isomers represented by the following general formula (Id). Specific examples of such compounds include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.
[0090]
[0091] The alicyclic dihydroxy compound represented by the general formula (I) includes: 1 Various isomers represented by the following general formula (Ie). Specific examples of such compounds include 1,3-adamantanedimethanol.
[0092]
[0093] Cyclohexanediol as the alicyclic dihydroxy compound represented by the general formula (II) includes R 2 The following general formula (IIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. ) represents various isomers. Specific examples of such compounds include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.
[0094]
[0095] The tricyclodecanediol or pentacyclopentadecanediol as the alicyclic dihydroxy compound represented by the general formula (II) comprises R 2 Various isomers represented by the following general formula (IIb) (wherein n represents 0 or 1).
[0096]
[0097] The alicyclic dihydroxy compound represented by the general formula (II) is decalinediool or tricyclotetradecanediol, which contains R 2 Various isomers represented by the following general formula (IIc) (wherein m represents 0 or 1). Specific examples of such compounds include 2,6-decalinediol, 1,5-decalinediol, and 2,3-decalinediol.
[0098]
[0099] Norbornanediol as the alicyclic dihydroxy compound represented by the general formula (II) includes R 2 Various isomers represented by the following general formula (IId). Specific examples of such compounds include 2,3-norbornanediol and 2,5-norbornanediol.
[0100]
[0101] The alicyclic dihydroxy compound represented by the general formula (II) includes: 2 Various isomers represented by the following general formula (IIe). Specific examples of such compounds include 1,3-adamantanediol.
[0102]
[0103] Specific examples of the alicyclic dihydroxy compounds include preferably cyclohexanedimethanols, tricyclodecanedimethanols, adamantanediols, and pentacyclopentadecanedimethanols. From the viewpoint of easy availability and easy handling, more preferably 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecanedimethanol. Still more preferably, tricyclodecanedimethanol is used.
[0104] The proportion of the structural units derived from the dihydroxy compound (B) relative to the structural units derived from all dihydroxy compounds contained in the PC-based resin is, for example, 0 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, and further preferably 30 mol% or more. On the other hand, the proportion of the structural units derived from the dihydroxy compound (B) is, for example, 90 mol% or less, preferably 60 mol% or less, and more preferably 40 mol% or less.
[0105] The details of these PC-based resins are described in, for example, Japanese Patent Application Laid-Open No. 2012-31370 (Patent No. 5448264), and the description of this patent document is incorporated herein by reference.
[0106] In one embodiment, the PC-based resin comprises a structural unit derived from a dihydroxy compound (A) represented by the above formula (2), a structural unit derived from an alicyclic dihydroxy compound (B) represented by the above general formula (I), and a carbonate group linking them. When the PC-based resin containing these structural units is applied to a substrate film, rainbow spots of the substrate film in optical inspection can be more stably suppressed.
[0107] In such a PC-based resin, the molar ratio (A:B) of the structural unit derived from the dihydroxy compound (A) represented by the above formula (2) to the structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I) is, for example, 5:5 to 9:1, and preferably 6:4 to 8:2.
[0108] In such a PC-based resin, the combination of the dihydroxy compound (A) represented by the above formula (2) and the alicyclic dihydroxy compound (B) represented by the above general formula (I) is preferably a combination of isosorbide and tricyclodecane dimethanol.
[0109] The substrate film 1 includes an AB agent in addition to a resin material. The AB agent preferably has transparency. As materials constituting the AB agent, for example, metal oxides, resins, and glass can be cited. As metal oxides, for example, silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, and calcium oxide can be cited. As resins, for example, polymethyl methacrylate, polystyrene, polyurethane, (meth) acrylic resin, (meth) acrylic acid-styrene copolymer, benzoguanamine, melamine, polycarbonate, and polysiloxane can be cited. As glass, for example, magnesium fluoride can be cited.
[0110] Any appropriate surface modification may be performed on the surface of the AB agent. Examples of the surface modification include chemical modification, and preferably alkyl modification.
[0111] The AB agents may be used alone or in combination of two or more.
[0112] Among such AB agents, preferably, metal oxides are used, more preferably, silica is used, further preferably, alkyl-modified silica is used, and particularly preferably, methyl-modified silica is used.
[0113] The substrate film 1 may contain any appropriate additives in addition to the above-mentioned resin material and AB agent. As additives, for example, antioxidants, ultraviolet absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents may be listed. Any appropriate surface treatment layer may be provided on the surface of the substrate film 1 (the surface on the opposite side of the adhesive layer 2). As surface treatment layers, for example, easy-adhesion layers, easy-slip layers, antistatic layers, antireflection layers, and anti-oligomer layers may be listed.
[0114] The thickness of the substrate film 1 is, for example, more than 30 μm, preferably more than 40 μm. On the other hand, the thickness of the substrate film 1 is, for example, less than 130 μm, preferably less than 120 μm. If the thickness of the substrate film is such a range, the substrate film can be given a toughness (elasticity) suitable for the peeling of the laminated film. Therefore, the substrate film can be peeled off smoothly from the adherend. In addition, the in-plane phase difference of the substrate film can be stably adjusted to the above-mentioned range.
[0115] The trouser tear strength of the substrate film 1 is, for example, 0.09N or more, preferably 0.10N or more. The trouser tear strength of the substrate film 1 is, for example, 0.4N or less, preferably 0.3N or less. If the trouser tear strength of the substrate film is within such a range, the laminated film can be smoothly peeled off from the adherend, and when the laminated film is peeled off from the adherend, rupture (cracking) can be suppressed on the laminated film. The trouser tear strength can be measured according to, for example, JIS K7128-1.
[0116] The total light transmittance of the base film 1 is, for example, 80% or more, preferably 85% or more, more preferably 90% or more, and further preferably 95% or more.
[0117] The haze value of the substrate film 1 is, for example, 2.0% or less, preferably 1.5% or less, more preferably 1.0% or less, further preferably 0.7% or less, particularly preferably 0.5% or less, and particularly preferably 0.3% or less. The lower limit of the haze value of the substrate film 1 is typically 0.05%.
[0118] When the total light transmittance and / or the haze value of the base film is within such a range, very excellent transparency can be imparted to the base film, and as a result, the influence of the laminated film in optical inspection of the adherend can be reduced.
[0119] C. Adhesive layer
[0120] The adhesive layer 2 is provided on the surface of the base film 1 in order to attach the laminated film 100 to the surface of an adherend. The adhesive layer 2 is made of an adhesive (pressure-sensitive adhesive).
[0121] As the adhesive constituting the adhesive layer 2, for example, (meth) acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives can be cited. By adjusting the type, quantity, combination, and proportion of the monomers forming the base resin of the adhesive, as well as the amount of the cross-linking agent, the reaction temperature, the reaction time, etc., an adhesive having desired properties corresponding to the purpose can be prepared. The base resin of the adhesive can be used alone or in combination of two or more.
[0122] In one embodiment, the adhesive layer 2 is made of a (meth)acrylic adhesive (a (meth)acrylic adhesive composition). If the adhesive layer is made of a (meth)acrylic adhesive, the peeling force of the laminated film can be stably adjusted to the above range.
[0123] The (meth)acrylic acid adhesive composition typically contains a (meth)acrylic acid polymer as a main component. The content of the (meth)acrylic acid polymer in the solid content of the adhesive composition is, for example, 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more. On the other hand, the upper limit of the content of the (meth)acrylic acid polymer is typically 100% by mass.
[0124] The (meth)acrylic polymer contains structural units derived from alkyl (meth)acrylate. In the (meth)acrylic polymer, the content of the structural units derived from alkyl (meth)acrylate is, for example, 70% by mass or more, preferably 80% by mass or more. On the other hand, the upper limit of the content of the structural units derived from alkyl (meth)acrylate is typically 90% by mass.
[0125] As the alkyl group of the (meth)acrylic acid alkyl ester, for example, a linear or branched alkyl group having 1 to 18 carbon atoms can be cited. The average number of carbon atoms in the alkyl group is preferably 3 to 12, more preferably 3 to 8. Among the (meth)acrylic acid alkyl esters, butyl acrylate and 2-ethylhexyl acrylate can be cited preferably, and 2-ethylhexyl acrylate can be cited more preferably.
[0126] The (meth)acrylic polymer may contain a structural unit derived from a comonomer polymerizable with the (meth)acrylic acid alkyl ester in addition to the structural unit derived from the (meth)acrylic acid alkyl ester. Examples of the comonomer include carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, aromatic ring-containing (meth)acrylic esters, and heterocyclic vinyl monomers. The comonomers may be used alone or in combination.
[0127] Among the comonomers, preferably, there are mentioned carboxyl group-containing monomers and hydroxyl group-containing monomers.
[0128] In one embodiment, the (meth)acrylic polymer includes a structural unit derived from an alkyl (meth)acrylate, a structural unit derived from a carboxyl group-containing monomer, and a structural unit derived from a hydroxyl group-containing monomer.
[0129] The carboxyl group-containing monomer is a compound containing a carboxyl group in its structure and containing polymerizable unsaturated double bonds such as a (meth)acryloyl group and a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, and crotonic acid, and preferably (meth)acrylic acid. When the (meth)acrylic acid polymer contains a structural unit derived from the carboxyl group-containing monomer, the adhesive properties of the adhesive layer can be improved.
[0130] When (meth) acrylic acid polymer contains the structural unit from carboxyl-containing monomer, the containing ratio of the structural unit from carboxyl-containing monomer is, for example, more than 0.01% by mass, preferably more than 0.10% by mass. On the other hand, the containing ratio of the structural unit from carboxyl-containing monomer is, for example, less than 10% by mass, preferably less than 5.0% by mass, more preferably less than 1.0% by mass, and further preferably less than 0.5% by mass.
[0131] Hydroxyl-containing monomers are compounds containing hydroxyl groups in their structures and containing polymerizable unsaturated double bonds such as (meth)acryloyl groups and vinyl groups. As hydroxyl-containing monomers, for example, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)-methacrylate can be listed, preferably 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate can be listed, and more preferably 4-hydroxybutyl (meth)acrylate can be listed. When the (meth)acrylic polymer contains a structural unit from a hydroxyl-containing monomer, the durability of the adhesive layer can be improved.
[0132] When the (meth)acrylic acid polymer contains a structural unit derived from a hydroxyl-containing monomer, the content of the structural unit derived from the hydroxyl-containing monomer is, for example, 0.01% by mass or more, preferably 1.0% by mass or more, more preferably 5.0% by mass or more, and further preferably 8.0% by mass or more. The upper limit of the content of the structural unit derived from the hydroxyl-containing monomer is typically 10% by mass.
[0133] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, 100,000 to 2,000,000, and preferably 200,000 to 1,000,000. The weight average molecular weight Mw can be calculated, for example, from the result of GPC measurement in terms of styrene.
[0134] In addition, the (meth)acrylic adhesive may contain a crosslinking agent. As the crosslinking agent, organic crosslinking agents and multifunctional metal chelates can be representatively listed, and preferably organic crosslinking agents can be listed. As the organic crosslinking agent, for example, isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents can be listed, and more preferably isocyanate crosslinking agents can be listed.
[0135] The content of the crosslinking agent is, for example, 0.01 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and further preferably 1.2 parts by mass or more relative to 100 parts by mass of the (meth) acrylic acid polymer. On the other hand, the content of the crosslinking agent is, for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 2.5 parts by mass or less, and further preferably 2.0 parts by mass or less. If the content of the crosslinking agent is within such a range, the peeling force of the laminated film can be appropriately adjusted.
[0136] The (meth)acrylic pressure-sensitive adhesive may contain various additives (eg, a silane coupling agent, a polymerization initiator, a solvent, and a cross-linking catalyst) at appropriate ratios.
[0137] The details of these adhesives are described in, for example, Japanese Patent Application Publication No. 2006-183022, Japanese Patent Application Publication No. 2015-199942, Japanese Patent Application Publication No. 2018-053114, Japanese Patent Application Publication No. 2016-190996, and International Publication No. 2018 / 008712, and the contents of these publications are incorporated herein by reference.
[0138] The thickness of the adhesive layer 2 is typically 1 μm or more, and preferably 5 μm or more. On the other hand, the thickness of the adhesive layer 2 is, for example, 30 μm or less, and preferably 15 μm or less.
[0139] The storage modulus of the adhesive layer 2 at 25° C. is, for example, 5.0×10 4 Pa~5.0×10 6 Pa, preferably 7.5×10 4 Pa~2.5×10 6 Pa. When the storage elastic modulus of the pressure-sensitive adhesive layer is within such a range, the wettability to the adherend is good and the adhesive force can be sufficient.
[0140] D. Release liner
[0141] The laminated film 100 may further include a release liner 3 in addition to the base film 1 and the adhesive layer 2. The release liner 3 is typically temporarily bonded to the adhesive layer 2 until the laminated film is attached to the adherend, and is peeled off from the adhesive layer 2 when the laminated film is attached. The release liner 3 is formed of any appropriate resin film that can be used as a release liner. A release treatment layer may also be provided on the contact surface of the release liner 3 with the adhesive layer 2.
[0142] E. Method for producing laminated film
[0143] The laminated film 100 can be manufactured by any appropriate method. In one embodiment, the manufacturing method of the laminated film includes: a step of preparing a resin composition (preparation step); a step of passing the resin composition through a filter (filter passing step); a step of extruding the resin composition after passing through the filter to prepare a substrate film 1 (extrusion molding step); and a step of forming an adhesive layer 2 on the substrate film 1 (adhesive layer forming step).
[0144] In the preparation step, typically, the resin material is melted, and then the molten resin material is mixed with the AB agent to prepare a resin composition.
[0145] The resin material before melting may have any appropriate shape. In one embodiment, the resin material may be granulated (granulated) in advance. The granulation method of the resin material is not particularly limited, and may be a wire cutting method or a thermal cutting method. The details of the pellet preparation process are recorded, for example, in Japanese Patent Publication No. 2013-181105. The description of this patent document is cited as a reference in this specification.
[0146] Next, the resin material (representatively, pellets) is heated to melt. The heating temperature can be any appropriate value corresponding to the resin material. In addition, the molten resin material is mixed with the AB agent. Thus, a molten resin composition is prepared. The range of the content ratio of the AB agent in the resin composition is, for example, the same as the range of the content ratio of the AB agent in the above-mentioned substrate film 1.
[0147] In the filter passing step, the molten resin composition is passed through a filter, thereby removing foreign matter and / or aggregates of the AB agent contained in the resin composition from the resin composition.
[0148] The filter may adopt any appropriate structure. Examples of the filter include a mesh and a disc filter, and preferably a mesh.
[0149] The mesh size of the screen is, for example, 0.080 mm or less, preferably 0.070 mm or less, and more preferably 0.055 mm or less. If the screen has such a mesh size, it is possible to prevent foreign matter and / or AB agent aggregates having a maximum Feret diameter of 30 μm or more from being mixed into the substrate film to be formed. Therefore, it is possible to reduce defects in the substrate film (specifically, foreign matter and / or AB agent aggregates), and it is possible to stably adjust the D30 / 10 cm of the substrate film. 2 Adjust to the above range.
[0150] On the other hand, the mesh size of the screen is, for example, 0.025 mm or more, preferably 0.035 mm or more. If the screen has such a mesh size, the resin composition can pass through the screen smoothly. Therefore, the retention of the resin composition can be suppressed, and the excessive heating of the resin composition can be suppressed. Thus, the occurrence of gel-like substances caused by the thermal crosslinking of the resin material can be suppressed. As a result, the defects in the substrate film (specifically, the gel-like substances) can be reduced, and the D30 / 10cm of the substrate film can be more stably increased. 2 Adjust to the above range.
[0151] In the extrusion molding step, the molten resin after passing through the filter is typically extruded into a film shape using a die, thereby preparing the base film 1. The above-mentioned preparation step, filter passing step and extrusion molding step can be carried out by any appropriate thin film forming apparatus.
[0152] Next, in the adhesive layer forming step, an adhesive layer 2 is formed on the obtained base film 1. As a method for forming the adhesive layer, any appropriate means can be adopted. In order to form the adhesive layer 2 on the base film 1, for example, the above-mentioned adhesive can be directly applied on the base film 1, or the adhesive can be applied on another base material to form the adhesive layer, and then transferred to the base film 1.
[0153] The method for producing a laminated film may further include a release liner attaching step and a winding step in addition to the above-mentioned preparation step, the above-mentioned film forming step and the above-mentioned adhesive layer forming step.
[0154] In the release liner sticking step, the release liner 3 is stuck to the surface of the adhesive layer 2 opposite to the base film 1 by any appropriate means. Then, in the winding step, the winding member winds the laminated film 100 to which the release liner 3 is stuck into a roll. The winding member typically has a cylindrical shape and can rotate around an axis.
[0155] Since the laminate film 100 has excellent anti-blocking properties, even when the laminate film 100 is wound into a roll and the base film 1 and the release liner 3 come into contact with each other, sticking of the base film 1 and the release liner 3 can be sufficiently suppressed.
[0156] As described above, the laminated film 100 is manufactured.
[0157] F. Application of laminated films
[0158] The laminated films described in the above sections A to E are used by being attached to the surfaces of various adherends. In one embodiment, the laminated film 100 is attached to the surface of the adherend via the adhesive layer 2 after the release liner 3 is peeled off from the adhesive layer 2 .
[0159] As adherends, for example, optical components and electronic components can be listed, and preferably optical components can be listed. As optical components, representative examples include polarizing plates, phase difference films, optical laminates including polarizing plates and / or phase difference films, displays, camera devices, lenses, and (half) mirrors.
[0160] In one embodiment, the laminated film 100 is a film with an adhesive layer, and can be used as a surface protective film. In this case, the laminated film 100 is attached to the surface of the adherend, and can protect the surface of the adherend during inspection, processing and / or transportation of the adherend.
[0161] Figure 2 is included Figure 1Schematic cross-sectional view of an optical component with a laminated film. The optical component with a laminated film 200 shown in the figure includes an optical component 5 as an adherend and a laminated film 100 as a surface protective film. The laminated film 100 is attached to the surface of the optical component 5 via an adhesive layer 2.
[0162] In one embodiment, the optical component 5 included in the optical component with a laminated film 200 is a polarizing plate. The thickness of the polarizing plate is, for example, 5 μm to 200 μm.
[0163] The thickness of the base film 1 of the laminated film 100 is, for example, 0.1 to 1.05, preferably 0.15 to 1.0, relative to the thickness of the adherend (optical component). If the thickness ratio of the base film to the adherend is within such a range, the adherend (optical component) can be inspected with better accuracy even when the laminated film is attached to the adherend for optical inspection.
[0164] Such an optical component 200 with a laminated film is typically used for optical inspection.
[0165] The optical inspection is not particularly limited, and for example, automatic optical inspection (AOI) can be cited. For example, the automatic optical inspection includes foreign matter inspection for inspecting foreign matter contained in optical components and bubble inspection for inspecting bubbles contained in optical components. In such optical inspection, since false detection caused by the laminate film (typically AB agent) is fully suppressed, the optical component can be inspected with good accuracy even when the laminate film is attached to the optical component.
[0166] Then, the laminated film 100 can be peeled off and removed from the surface of the optical component 5 at a desired timing.
[0167] Example
[0168] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. It should be noted that the measuring methods of the various properties are as follows.
[0169] (1) Determination of the number of defects in the substrate film
[0170] The substrate films used in Examples and Comparative Examples were measured using an optical microscope for a unit area of 10 cm. 2 The results are shown in Table 1.
[0171] (2) Rainbow spots on the substrate film
[0172] The substrate film used in the examples and comparative examples was placed between two polarizing plates in a crossed Nicol state. At this time, the substrate film was placed so that the length direction of the substrate film was parallel to the transmission axis direction of one polarizing plate. In this state, the light of a fluorescent lamp was irradiated from the lower side of the lower polarizing plate, and the presence or absence of rainbow spots was visually observed. The results are shown in Table 1.
[0173] (3) Automatic foreign body inspection
[0174] Regarding the laminated films obtained in Examples and Comparative Examples, the number of foreign matter contained in an area of 10 cm×10 cm in the laminated films was counted based on the method described in Japanese Patent Application Laid-Open No. 2021-135219.
[0175] Next, the results of the automatic foreign matter inspection were evaluated according to the following criteria, and the results are shown in Table 1.
[0176] ○: The number of foreign matter larger than 30 μm is 5 / 10 cm 2 the following
[0177] ×: The number of foreign matter larger than 30 μm is 6 to 10 pieces / 10 cm 2 above
[0178] ××: The number of foreign matter larger than 30 μm is 11 pieces / 10 cm 2 above
[0179] (4) Sliding properties (anti-adhesion properties)
[0180] The base films of the laminated films obtained in Examples and Comparative Examples were rubbed against each other, and the sliding property (anti-blocking property) was evaluated according to the following criteria. The results are shown in Table 1.
[0181] ◎: The substrate films do not stick to each other and slide well
[0182] ○: The substrate films do not stick to each other, but are slightly slippery compared to ◎
[0183] ×: The base films are together and do not slide
[0184] <<Preparation Example 1: Adhesive composition>>
[0185] In a reaction container equipped with a thermometer, a stirrer, a cooler and a nitrogen inlet pipe, 100 parts by mass of 2-ethylhexyl acrylate (2EHA) as a monomer component, 10 parts by mass of 4-hydroxybutyl acrylate (4HBA), 0.02 parts by mass of acrylic acid (AA) and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were placed together with 157 parts by mass of ethyl acetate, and nitrogen was introduced while slowly stirring at 23°C to perform nitrogen replacement. Then, the liquid temperature was maintained at around 65°C, and a polymerization reaction was performed for 6 hours to prepare a solution of (meth)acrylate polymer A (concentration 40% by mass). The weight average molecular weight of acrylate polymer A was 540,000.
[0186] Ethyl acetate was added to the solution of the acrylic polymer A to dilute it to a concentration of 20 mass %. To 500 mass parts (100 mass parts of solid content) of this solution, 1.5 mass parts of isocyanurate of 1,6-hexanediisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 mass parts (0.03 mass parts of solid content) of dibutyltin dilaurate (1 mass % ethyl acetate solution) as a crosslinking catalyst were added and stirred to prepare an adhesive composition.
[0187] <<Preparation Example 2: PC-based resin film>>
[0188] Relative to 81.98 mass parts of isosorbide (ISB), 47.19 mass parts of tricyclodecane dimethanol (TCDDM), 175.1 mass parts of diphenyl carbonate (DPC) and 0.979 mass parts of cesium carbonate 0.2 mass % aqueous solution as catalyst are put into reaction vessel, under nitrogen atmosphere, as the first stage of reaction, heating tank temperature is heated to 150 ℃, while stirring as required, raw materials are dissolved (about 15 minutes). Then, the pressure is made from normal pressure to 13.3kPa, while the heating tank temperature is raised to 190 ℃ in 1 hour, the phenol produced is discharged outside the reaction vessel. After the reaction vessel as a whole is kept at 190 ℃ for 15 minutes, as the second stage of operation, the pressure in the reaction vessel is 6.67kPa, the heating tank temperature is raised to 230 ℃ in 15 minutes, and the phenol produced is discharged outside the reaction vessel. As the stirring torque of the stirrer continued to increase, the temperature was raised to 250°C in 8 minutes, and the pressure in the reaction container was reduced to below 0.200 kPa in order to further remove the generated phenol. After reaching the specified stirring torque, the reaction was terminated, and the generated reactants were extruded into water to obtain PC resin pellets.
[0189] [Example 1, Comparative Examples 2 and 3]
[0190] The pellets of the PC resin obtained in Preparation Example 2 were vacuum dried at 100° C. for 12 hours. Then, the pellets of the PC resin and the AB agent (microparticles obtained by methyl-modifying silica, primary particle size: 0.5 μm, manufactured by Nippon Catalyst Co., Ltd., trade name: SEAHOSTAR KE) were supplied to a thin film forming device. The addition ratio of the AB agent to the total amount of the pellets and the AB agent, and the primary particle size of the AB agent are shown in Table 1.
[0191] The film forming apparatus includes: a single screw extruder (manufactured by Toshiba Machine Co., Ltd., barrel setting temperature: 250°C), a screen with a mesh size of 0.045 mm, a T-die (width 1700 mm, setting temperature: 250°C), a chilled casting roll (setting temperature: 60°C) and a winder.
[0192] More specifically, the pellets and the AB agent are supplied to a single screw extruder for heating. As a result, the pellets are melted, and the molten PC resin and the AB agent are kneaded to prepare a resin composition. Then, the resin composition is extruded from the single screw extruder and passes through a screen and a T-die in sequence. Thus, a PC resin film with a thickness of 40 μm is formed. After passing through a cold casting roll, the PC resin film is wound using a winder.
[0193] Next, the adhesive composition of Preparation Example 1 was applied to the release-treated surface of a release liner (a biaxially stretched polyethylene terephthalate film having a thickness of 25 μm after silicone release treatment on one side), and heated at 130° C. for 20 seconds to form an adhesive layer having a thickness of 10 μm. The adhesive layer was bonded to the corona-treated surface of a PC-based resin film having a corona treatment on one side to obtain a laminated film.
[0194] [Example 2]
[0195] A laminated film was obtained by performing the same operation as in Example 1 except that the AB agent (microparticles obtained by subjecting silica to methyl modification, with an average primary particle size of 0.5 μm, manufactured by Nippon Catalyst Co., Ltd., trade name: SEAHOSTAR KE) was changed to AB agent (microparticles obtained by subjecting silica to methyl modification, with an average primary particle size of 1.0 μm, manufactured by Nippon Catalyst Co., Ltd., trade name: SEAHOSTAR KE).
[0196] [Example 3]
[0197] A laminated film was obtained in the same manner as in Example 1 except that the pellets of the PC-based resin obtained in Preparation Example 2 were changed to pellets of a COP-based resin.
[0198] [Comparative Example 1]
[0199] A laminated film was obtained by performing the same operation as in Example 1 except that the AB agent (microparticles obtained by methyl-modifying silica, with an average primary particle size of 0.5 μm, manufactured by Nippon Catalyst Co., Ltd., trade name: SEAHOSTAR KE) was changed to AB agent (microparticles obtained by methyl-modifying silica, with an average primary particle size of 1.5 μm, manufactured by Nippon Catalyst Co., Ltd., trade name: SEAHOSTAR KE).
[0200] Table 1
[0201]
[0202] [evaluate]
[0203] As can be seen from Table 1, when the content ratio of the AB agent in the base film is 350 ppm or more, the laminated film has excellent anti-adhesion properties. In addition, when the content ratio of the AB agent in the base film is 3000 ppm or less and the average primary particle size of the AB agent is 1.3 μm or less, even when the laminated film is attached to an adherend and subjected to optical inspection, false detection caused by the AB agent can be suppressed, thereby enabling the adherend to be inspected with good accuracy.
[0204] Industrial Applicability
[0205] The laminated film of the present invention can be applied to various industrial products, and can be suitably used in optical products used for optical inspection in particular.
Claims
1. A laminated film comprising a substrate film and an adhesive layer laminated on the substrate film, The substrate film comprises a resin material as a matrix and an anti-blocking agent dispersed in the resin material, The average primary particle size of the anti-blocking agent is 1.3 μm or less, The content ratio of the anti-blocking agent in the base film is 350 ppm to 3000 ppm.
2. The laminated film according to claim 1, wherein The unit area of the substrate film is 10 cm 2 The number of defects having a maximum Feret diameter of 30 μm or more is 5 or less.
3. The laminated film according to claim 1 or 2, wherein The in-plane retardation Re (550) of the substrate film is 10 nm or less.
4. The laminated film according to claim 1 or 2, wherein The base film has a dynamic friction coefficient of 1.0 or less. 5 . The laminated film according to claim 1 , wherein the peeling force to a polyacrylate plate at a tensile speed of 30 m / min and a peeling angle of 180° is 3.0 N / 25 mm or less.
6. The laminated film according to claim 1 or 2, wherein The resin material includes a polycarbonate-based resin and / or a cycloolefin-based resin.
7. A method for manufacturing a laminated film, comprising: A step of mixing a molten resin material with an anti-blocking agent to prepare a resin composition; The step of passing the resin composition through a filter; A step of extruding the resin composition after passing through the filter to prepare a substrate film; and forming an adhesive layer on the substrate film, The average primary particle size of the anti-blocking agent is 1.3 μm or less, The content ratio of the anti-blocking agent in the resin composition is 350 ppm to 3000 ppm.
8. The method for producing a laminated film according to claim 7, wherein: The filter is a sieve, and the mesh size of the sieve is 0.035 mm to 0.070 mm.