Composite silk screen and preparation method thereof, silk screen printing device and camera lens

By introducing vertically woven polyester threads and annular hot-melt adhesive layers into the stainless steel screen, the problem of deformation of the stainless steel screen during long-term use is solved, and high-precision and long-life screen printing effects are achieved.

CN118721963AInactive Publication Date: 2024-10-01CHIZHOU RUIOU OPTICAL TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410968031.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing stainless steel screens are prone to plastic deformation after long-term use, resulting in reduced printing accuracy and insufficient service life, making it difficult to meet the needs of high-precision pattern printing.

Method used

A composite screen printing screen is used. Stainless steel wires and polyester wires are woven vertically to form an intermediate screen. The polyester wires extending in the direction of scraper movement provide elastic support. The annular hot melt adhesive layer and polyester mesh are combined to improve the screen printing performance. Stability and service life.

Benefits of technology

While achieving high-precision pattern printing, it also extends the service life of the screen, avoids the deformation problem of the stainless steel screen during long-term use, and improves the printing accuracy and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721963A_ABST
    Figure CN118721963A_ABST
Patent Text Reader

Abstract

In order to solve the problem that the printing precision is affected by plastic deformation of an existing stainless steel silk screen after long-time use, the invention provides a composite silk screen which is used for being matched with a scraper for silk-screen printing and comprises a middle screen printing plate, the middle screen printing plate comprises a plurality of stainless steel wires and a plurality of polyester wires, the stainless steel wires are arranged in parallel, and the polyester wires are arranged in parallel. The stainless steel wires and the polyester wires are arranged in parallel, the polyester wires extend in the moving direction of the scraper, the stainless steel wires are perpendicular to the polyester wires, and the stainless steel wires and the polyester wires are woven to form a net structure. Meanwhile, the invention further discloses a preparation method of the composite silk screen, a silk screen printing device and a camera lens. The composite silk screen provided by the invention can realize higher printing precision control, and is suitable for printing operation of high-precision patterns; and the deformation of the middle screen printing plate after long-term use can be effectively inhibited, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of camera lens preparation, and in particular relates to a composite silk screen screen and a preparation method thereof, a silk screen printing device, and a camera lens. Background Art

[0002] In the process of preparing camera lenses, black ink is usually printed on the peripheral area of ​​the camera to avoid the influence of stray light on the camera image acquisition, and at the same time, it also has a shielding effect on the peripheral structure of the camera to improve the aesthetics. The ink printing of existing camera lenses is usually carried out by silk screen printing. On some camera lenses that do not require high pattern accuracy, polyester silk screen and polyurethane silk screen are mainly used for printing. The advantage is that the material cost is relatively low. At the same time, since polyester and polyurethane have good elasticity, they can adapt to the reciprocating motion of the scraper and produce elastic deformation. They have high fatigue resistance and long service life. However, polyester silk screen and polyurethane silk screen cannot be used on some camera lenses that require high printing pattern accuracy. For example, for mirror silver characters and CD pattern silk screen printing below 0.1*0.1mm, the mesh accuracy of conventional polyester silk screen and polyurethane silk screen is difficult to meet the printing requirements. The strength and precision of the stainless steel screen can meet the requirements of high-precision pattern printing, but the elasticity of the stainless steel screen is poor. During the screen printing process, it is easy to produce fatigue deformation and plastic deformation due to force, which makes it difficult for the screen to maintain its tension and return to its original position, resulting in deformation of the printed pattern and insufficient service life. An existing solution is to fix the stainless steel screen in the middle of the polyester screen, and use the high elasticity of the polyester screen to alleviate the deformation of the stainless steel screen during the operation of the scraper. However, although this method improves the service life to a certain extent, it cannot completely solve the problem of the plastic deformation of the stainless steel screen. In particular, the stainless steel wire in the stainless steel screen that is consistent with the running direction of the scraper is severely deformed during long-term use. Summary of the invention

[0003] In view of the problem that the existing stainless steel screen suffers from plastic deformation and affects the printing accuracy after long-term use, the present invention provides a composite screen printing screen and a preparation method thereof, a screen printing device, and a camera lens.

[0004] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0005] On the one hand, the present invention provides a composite screen printing mesh for screen printing in cooperation with a scraper, including an intermediate screen plate, wherein the intermediate screen plate includes a plurality of stainless steel wires and a plurality of polyester wires, the plurality of stainless steel wires are arranged parallel to each other, the plurality of polyester wires are arranged parallel to each other, the polyester wires extend along the movement direction of the scraper, and the stainless steel wires are perpendicular to the polyester wires, and the plurality of stainless steel wires and the plurality of polyester wires are woven together to form a mesh structure.

[0006] Optionally, the diameter of the polyester wire is 30-60 μm, and the diameter of the stainless steel wire is 6-20 μm.

[0007] Optionally, nanopores are formed on the surface of the stainless steel wire, and there is an intersection between the stainless steel wire and the polyester wire. At the intersection, the polyester wire and the stainless steel wire are bonded to each other, and a portion of the polyester wire enters the nanopores.

[0008] Optionally, it also includes a screen frame and a polyester screen, wherein the polyester screen is an annular screen surrounding the outer circumference of the intermediate screen, the inner edge of the polyester screen is connected to the outer edge of the intermediate screen, and the outer edge of the polyester screen is fixed to the screen frame.

[0009] Optionally, an annular hot melt adhesive layer is further included, the inner edge of the polyester mesh is overlapped with the outer edge of the intermediate screen, and the annular hot melt adhesive layer is located at the overlapping portion of the polyester mesh and the intermediate screen to fix the polyester mesh and the intermediate screen layer.

[0010] In another aspect, the present invention provides a method for preparing the composite screen printing mesh as described above, comprising the following operations:

[0011] A plurality of stainless steel wires and a plurality of polyester wires are interlaced and woven, wherein the plurality of stainless steel wires are arranged parallel to each other, the plurality of polyester wires are arranged parallel to each other, and the stainless steel wires and the polyester wires are perpendicular to each other, so as to form an intermediate screen;

[0012] A composite screen printing screen is produced by using the intermediate screen plate.

[0013] Optionally, the stainless steel wire is subjected to etching pretreatment before braiding, and the etching pretreatment includes the following operations:

[0014] The stainless steel wire is unwound and sequentially pulled through a first acid solution, a first cleaning tank, a second acid solution and a second cleaning tank, and then rewound;

[0015] Wherein, the first acid solution comprises hydrochloric acid, sulfuric acid, copper sulfate and water, the concentration of the hydrochloric acid is 50-120 g / L, the concentration of the sulfuric acid is 60-150 g / L, and the concentration of the copper sulfate is 1-10 g / L; the second acid solution comprises sodium fluoride, oxalic acid and water, the concentration of the sodium fluoride is 10-20 g / L, and the concentration of the oxalic acid is 10-50 g / L.

[0016] Optionally, the process of making a composite screen printing screen from the intermediate screen plate includes the following operations:

[0017] The middle screen is placed on the surface of the first polytetrafluoroethylene plate, the polyester mesh is placed on the periphery of the middle screen, the inner edge of the polyester mesh is overlapped with the outer edge of the middle screen, the annular hot melt adhesive layer is placed on the overlapped portion of the polyester mesh and the middle screen, the second polytetrafluoroethylene plate is covered and hot pressed, the hot pressing range covers the middle screen and the annular hot melt adhesive layer, the hot pressing temperature is 230° C. to 250° C., the pressure is 3 to 5 MPa, at the intersection of the stainless steel wire and the polyester wire, the polyester wire is partially hot-melted and enters the nanopores on the surface of the stainless steel wire;

[0018] After hot pressing, the mesh is cooled to room temperature, and the outer edge of the cooled polyester mesh is assembled and fixed with the mesh frame to obtain a composite screen printing mesh.

[0019] In yet another aspect, the present invention provides a screen printing device comprising a scraper and the composite screen as described above.

[0020] On the other hand, the present invention provides a camera lens, comprising a lens and an ink layer, wherein the ink layer is obtained by silk screen printing, and the silk screen printing adopts the silk screen printing device as described above.

[0021] According to the composite silk screen mesh provided by the present invention, stainless steel wire and polyester wire are woven together to form an intermediate screen, and the polyester wire extends along the movement direction of the scraper. On the one hand, the composite silk screen mesh has high strength through the stainless steel wire therein, can meet the requirements of silk screen printing, can achieve high printing accuracy control, and is suitable for printing operations of high-precision patterns; on the other hand, because the polyester wire extends along the movement direction of the scraper, when the scraper moves, the elasticity of the polyester wire can adapt to the movement of the scraper to produce reversible deformation, thereby effectively suppressing the deformation of the intermediate screen under long-term use and improving the service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the structure of the composite screen printing mesh provided by the present invention;

[0023] Figure 2 is an enlarged schematic diagram of the intermediate screen provided by the present invention;

[0024] Figure 3It is a schematic structural diagram of the intermediate screen before hot pressing provided by the present invention;

[0025] Figure 4 It is a schematic diagram of the structure of the intermediate screen after hot pressing provided by the present invention.

[0026] The reference numerals in the drawings of the specification are as follows:

[0027] 1. Middle screen; 11. Polyester wire; 12. Stainless steel wire; 2. Polyester mesh; 3. Screen frame; 4. Annular hot melt adhesive layer. DETAILED DESCRIPTION

[0028] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0029] See also Figure 1 and Figure 2 As shown, an embodiment of the present invention provides a composite screen printing mesh for performing screen printing in cooperation with a scraper, comprising an intermediate screen plate 1, wherein the intermediate screen plate 1 comprises a plurality of stainless steel wires 12 and a plurality of polyester wires 11, wherein the plurality of stainless steel wires 12 are arranged parallel to each other, and the plurality of polyester wires 11 are arranged parallel to each other, wherein the polyester wires 11 extend along the movement direction of the scraper, and the stainless steel wires 12 and the polyester wires 11 are perpendicular to each other, and the plurality of stainless steel wires 12 and the plurality of polyester wires 11 are woven together to form a mesh structure.

[0030] The composite screen printing mesh uses stainless steel wires 12 and polyester wires 11 to weave together to form an intermediate screen 1, and the polyester wires 11 extend along the movement direction of the scraper. On the one hand, the composite screen printing mesh has high strength through the stainless steel wires therein, which can meet the requirements of screen printing, and can achieve high printing accuracy control, and is suitable for printing operations of high-precision patterns; on the other hand, since the polyester wires 11 extend along the movement direction of the scraper, when the scraper moves, the elasticity of the polyester wires 11 can adapt to the movement of the scraper to produce reversible deformation, thereby effectively suppressing the deformation of the intermediate screen 1 under long-term use and improving the service life.

[0031] In some embodiments, the diameter of the polyester wire 11 is 30-60 μm, and the diameter of the stainless steel wire 12 is 6-20 μm.

[0032] The polyester wire 11 has a larger diameter to ensure sufficient elasticity to adapt to the deformation of the scraper movement, and the stainless steel wire 12 has a smaller diameter to form a composite screen with smaller meshes to improve the screen printing accuracy.

[0033] In some embodiments, nanopores are formed on the surface of the stainless steel wire 12, and there is an intersection between the stainless steel wire 12 and the polyester wire 11. At the intersection, the polyester wire 11 and the stainless steel wire 12 are bonded to each other, and a portion of the polyester wire 11 enters the nanopores.

[0034] By bonding the polyester wire 11 and the stainless steel wire 12 to each other at the intersection, it is helpful to avoid relative displacement between the polyester wire 11 and the stainless steel wire 12 during the movement of the scraper, thereby improving the stability of the composite screen printing mesh, and also helping to make full use of the elasticity of the polyester wire 11 to restore the position of the stainless steel wire 12 after the scraper action point is transferred. Correspondingly, in order to improve the connection strength of the polyester wire 11 and the stainless steel wire 12 at the intersection, nanopores are formed on the surface of the stainless steel wire 12, and the polyester wire 11 is softened by hot pressing and partially penetrated into the nanopores, effectively improving the connection tightness between the polyester wire 11 and the stainless steel wire 12.

[0035] In some embodiments, the composite silk screen screen also includes a screen frame 3 and a polyester screen 2, wherein the polyester screen 2 is an annular screen surrounding the outer periphery of the intermediate screen plate 1, the inner edge of the polyester screen 2 is connected to the outer edge of the intermediate screen plate 1, and the outer edge of the polyester screen 2 is fixed on the screen frame 3.

[0036] The polyester mesh 2 is helpful to further improve the overall elasticity of the composite screen printing mesh. The intermediate screen 1 is used as a pattern setting screen, and the polyester mesh 2 plays an elastic supporting role to reduce the deformation of the intermediate screen 1 during the movement of the scraper, thereby playing a protective role for the intermediate screen 1.

[0037] In some embodiments, the composite silk screen screen also includes an annular hot melt adhesive layer 4, the inner edge of the polyester mesh 2 is overlapped with the outer edge of the intermediate screen 1, and the annular hot melt adhesive layer 4 is located at the overlapping part of the polyester mesh 2 and the intermediate screen 1 to fix the polyester mesh 2 and the intermediate screen 1 layer.

[0038] The annular hot melt adhesive layer 4 is used to fix the polyester mesh 2 and the intermediate screen plate 1 to prevent the two from being separated under the force of the scraper.

[0039] Another embodiment of the present invention provides a method for preparing the composite screen printing mesh as described above, comprising the following operations:

[0040] A plurality of stainless steel wires 12 and a plurality of polyester wires 11 are interlaced and woven, wherein the plurality of stainless steel wires 12 are arranged parallel to each other, the plurality of polyester wires 11 are arranged parallel to each other, and the stainless steel wires 12 and the polyester wires 11 are perpendicular to each other, so as to form an intermediate screen 1;

[0041] The composite screen printing screen is manufactured from the intermediate screen plate 1 .

[0042] In some embodiments, the stainless steel wire 12 is subjected to etching pretreatment before braiding, and the etching pretreatment includes the following operations:

[0043] The stainless steel wire 12 is unwound and sequentially pulled through the first acid solution, the first cleaning tank, the second acid solution and the second cleaning tank, and then rewound;

[0044] Wherein, the first acid solution comprises hydrochloric acid, sulfuric acid, copper sulfate and water, the concentration of the hydrochloric acid is 50-120 g / L, the concentration of the sulfuric acid is 60-150 g / L, and the concentration of the copper sulfate is 1-10 g / L; the second acid solution comprises sodium fluoride, oxalic acid and water, the concentration of the sodium fluoride is 10-20 g / L, and the concentration of the oxalic acid is 10-50 g / L.

[0045] The stainless steel wire 12 is subjected to preliminary surface etching and surface oxide removal treatment by the first acid solution. After being treated with the first acid solution, small nano-scale pits appear on the surface of the stainless steel wire 12. Then, the stainless steel wire 12 is cleaned in the first cleaning tank to remove the residual first acid solution. The cleaned stainless steel wire 12 enters the second acid solution again for secondary etching. The secondary etching can further etch based on the nano-scale small pits formed by the preliminary etching to obtain nano-scale holes. The stainless steel wire that has undergone the secondary etching enters the second cleaning tank for cleaning to remove the residual second acid solution on the surface.

[0046] In one embodiment, the first cleaning tank and the second cleaning tank are filled with water, and ultrasonic devices are provided in the first cleaning tank and the second cleaning tank to improve cleaning efficiency and avoid the first acid solution or the second acid solution remaining in the nano-scale pores.

[0047] In some embodiments, the composite screen printing screen is produced by the intermediate screen plate 1, including the following operations:

[0048] The intermediate screen 1 is placed on the surface of the first polytetrafluoroethylene plate, and the polyester mesh 2 is placed on the periphery of the intermediate screen 1. The inner edge of the polyester mesh 2 is overlapped with the outer edge of the intermediate screen 1. The annular hot melt adhesive layer 4 is placed on the overlapping part of the polyester mesh 2 and the intermediate screen 1, and the second polytetrafluoroethylene plate is covered and hot pressed. The hot pressing range covers the intermediate screen 1 and the annular hot melt adhesive layer 4. The hot pressing temperature is 230°C to 250°C, and the pressure is 3 to 5MPa. At the intersection of the stainless steel wire 12 and the polyester wire 11, the polyester wire 11 is partially hot-melted and enters the nanopores on the surface of the stainless steel wire 12.

[0049] like Figure 3As shown in FIG. 1 , the stainless steel wire 12 and the polyester wire 11 are formed before hot pressing. At this time, the polyester wire 11 is wavy, and the boundary between the stainless steel wire 12 and the polyester wire 11 is obvious, and there is no mutual adhesion. Figure 4 As shown, the stainless steel wire 12 and the polyester wire 11 are hot pressed. At this time, the polyester wire 11 tends to be flatter, and the stainless steel wire 12 is embedded in the polyester wire 11 to form a stable connection.

[0050] The first polytetrafluoroethylene plate and the second polytetrafluoroethylene plate are used to prevent the polyester wire 11, the annular hot melt adhesive layer 4 or the polyester mesh 2 from adhering to the hydraulic mold during the hot pressing process.

[0051] In some embodiments, the polyester mesh 2 is cooled to room temperature after hot pressing, and the outer edge of the cooled polyester mesh 2 is assembled and fixed to the mesh frame 3 to obtain a composite screen printing mesh.

[0052] Another embodiment of the present invention provides a screen printing device, comprising a scraper and the composite screen as described above.

[0053] It should be noted that when the composite silk screen is used in a silk screen printing device, it is necessary to pre-set the silk screen pattern on the intermediate screen 1. The silk screen pattern can be set in an existing way, such as by using photosensitive resin and exposing and developing to mask the composite silk screen in the non-silk screen pattern area, thereby retaining only the mesh holes of the composite silk screen at the silk screen pattern position to meet the ink penetration requirements of the silk screen pattern.

[0054] Another embodiment of the present invention provides a camera lens, comprising a lens and an ink layer, wherein the ink layer is obtained by silk screen printing, and the silk screen printing adopts the silk screen printing device as described above.

[0055] The present invention is further described below by way of examples.

[0056] Example 1

[0057] This embodiment is used to illustrate the composite screen printing mesh and the preparation method thereof disclosed in the present invention, and includes the following operations:

[0058] Stainless steel wire etching: A stainless steel wire with a diameter of 15 μm is used to perform etching pretreatment on the stainless steel wire: the stainless steel wire is unwound and sequentially pulled through the first acid solution, the first cleaning tank, the second acid solution and the second cleaning tank, and then rewound;

[0059] Wherein, the first acid solution includes hydrochloric acid, sulfuric acid, copper sulfate and water, the concentration of the hydrochloric acid is 70g / L, the concentration of the sulfuric acid is 100g / L, and the concentration of the copper sulfate is 3g / L; the second acid solution includes sodium fluoride, oxalic acid and water, the concentration of the sodium fluoride is 15g / L, and the concentration of the oxalic acid is 20g / L.

[0060] A plurality of stainless steel wires and a plurality of polyester wires are interlaced and woven, wherein the diameter of the polyester wire is 35 μm, the plurality of stainless steel wires are arranged parallel to each other, the plurality of polyester wires are arranged parallel to each other, and the stainless steel wires and the polyester wires are perpendicular to each other, so as to form an intermediate screen;

[0061] The intermediate screen is placed on the surface of the first polytetrafluoroethylene plate, and the polyester mesh is placed on the periphery of the intermediate screen. The inner edge of the polyester mesh is overlapped with the outer edge of the intermediate screen, and the annular hot melt adhesive layer is placed on the overlapping part of the polyester mesh and the intermediate screen. The second polytetrafluoroethylene plate is covered and hot pressed. The hot pressing range covers the intermediate screen and the annular hot melt adhesive layer. The hot pressing temperature is 240°C and the pressure is 4MPa.

[0062] After hot pressing, the mesh is cooled to room temperature, and the outer edge of the cooled polyester mesh is assembled and fixed with the mesh frame to obtain a composite screen printing mesh;

[0063] A CD silk screen pattern (multiple concentrically spaced circular ring patterns) is formed on the intermediate screen by using photosensitive resin and exposing and developing the pattern.

[0064] Example 2

[0065] This embodiment is used to illustrate the composite screen printing mesh and the preparation method thereof disclosed in the present invention, and includes most of the operations in Example 1, except that:

[0066] During the heat pressing, the heat pressing range only covers the annular hot melt adhesive layer, and does not cover the portion of the middle screen where the annular hot melt adhesive layer is not provided.

[0067] Example 3

[0068] This embodiment is used to illustrate the composite screen printing mesh and the preparation method thereof disclosed in the present invention, and includes most of the operations in Example 1, except that:

[0069] No etching of the stainless steel wire is performed, and smooth stainless steel wire and polyester thread are directly used for weaving.

[0070] Comparative Example 1

[0071] This comparative example is used to compare and illustrate the composite screen printing mesh disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0072] A stainless steel wire mesh is used to replace the middle screen in the embodiment.

[0073] Performance Testing

[0074] The composite screen printing mesh prepared above was subjected to the following performance tests:

[0075] The composite screen printing screen is installed on the screen printing device, black ink is added to the screen frame of the composite screen printing screen, a support plate is set at the bottom of the composite screen printing screen, and a scraper is used to move back and forth on the composite screen printing screen along the extension direction of the polyester line. Multiple support plates are recycled through cyclic cleaning and drying, and the number of reciprocating times of the scraper is recorded. After every 2000 operations, a glass sheet is placed at the bottom of the composite screen printing screen for CD grain screen printing, and the CD grain pattern is observed through a microscope. When CD grain texture defects appear, the current number of cycles and the texture defects that appear are recorded, and the test results obtained are filled in Table 1.

[0076] Table 1

[0077]

[0078] It can be seen from the test results in Table 1 that the composite screen printing mesh provided by the present invention can realize the printing of fine patterns (CD patterns), and at the same time, the service life is greatly improved compared with the conventional steel screen.

[0079] By comparing the test results of Examples 1 to 3, it can be seen that the etching treatment of the stainless steel wire and the subsequent hot pressing treatment can both improve the bonding strength between the polyester wire and the stainless steel wire, and ultimately increase their service life.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite screen printing net, used for screen printing in cooperation with a scraper, characterized in that: It includes an intermediate screen, which includes multiple stainless steel wires and multiple polyester wires. The multiple stainless steel wires are arranged in parallel with each other, and the multiple polyester wires are arranged in parallel with each other. The polyester wires extend along the movement direction of the scraper, and the stainless steel wires and the polyester wires are perpendicular to each other. The multiple stainless steel wires and the multiple polyester wires are woven together to form a mesh structure.

2. The composite screen printing mesh according to claim 1, characterized in that: The diameter of the polyester wire is 30-60 μm, and the diameter of the stainless steel wire is 6-20 μm.

3. The composite screen printing mesh according to claim 1, characterized in that: Nanopores are formed on the surface of the stainless steel wire. There is an intersection between the stainless steel wire and the polyester wire. At the intersection, the polyester wire and the stainless steel wire are bonded to each other, and a portion of the polyester wire enters the nanopores.

4. The composite screen printing mesh according to claim 1, characterized in that: It also includes a screen frame and a polyester screen. The polyester screen is an annular screen surrounding the outer periphery of the intermediate screen. The inner edge of the polyester screen is connected to the outer edge of the intermediate screen, and the outer edge of the polyester screen is fixed on the screen frame.

5. The composite screen printing mesh according to claim 4, characterized in that: It also includes an annular hot melt adhesive layer. The inner edge of the polyester mesh is overlapped with the outer edge of the intermediate screen. The annular hot melt adhesive layer is located at the overlapping portion of the polyester mesh and the intermediate screen to fix the polyester mesh and the intermediate screen layer.

6. The method for preparing a composite screen printing mesh according to any one of claims 1 to 5, characterized in that: The following operations are included: A plurality of stainless steel wires and a plurality of polyester wires are interlaced and woven, wherein the plurality of stainless steel wires are arranged parallel to each other, the plurality of polyester wires are arranged parallel to each other, and the stainless steel wires and the polyester wires are perpendicular to each other, so as to form an intermediate screen; A composite screen printing screen is produced by using the intermediate screen plate.

7. The method for preparing a composite screen printing mesh according to claim 6, characterized in that: The stainless steel wire is subjected to etching pretreatment before braiding, and the etching pretreatment includes the following operations: The stainless steel wire is unwound and sequentially pulled through a first acid solution, a first cleaning tank, a second acid solution and a second cleaning tank, and then rewound; Wherein, the first acid solution comprises hydrochloric acid, sulfuric acid, copper sulfate and water, the concentration of the hydrochloric acid is 50-120 g / L, the concentration of the sulfuric acid is 60-150 g / L, and the concentration of the copper sulfate is 1-10 g / L; the second acid solution comprises sodium fluoride, oxalic acid and water, the concentration of the sodium fluoride is 10-20 g / L, and the concentration of the oxalic acid is 10-50 g / L.

8. The method for preparing a composite screen printing mesh according to claim 7, characterized in that: The process of making a composite screen printing mesh from the intermediate screen includes the following operations: The middle screen is placed on the surface of the first polytetrafluoroethylene plate, the polyester mesh is placed on the periphery of the middle screen, the inner edge of the polyester mesh is overlapped with the outer edge of the middle screen, the annular hot melt adhesive layer is placed on the overlapped portion of the polyester mesh and the middle screen, the second polytetrafluoroethylene plate is covered and hot pressed, the hot pressing range covers the middle screen and the annular hot melt adhesive layer, the hot pressing temperature is 230° C. to 250° C., the pressure is 3 to 5 MPa, at the intersection of the stainless steel wire and the polyester wire, the polyester wire is partially hot-melted and enters the nanopores on the surface of the stainless steel wire; After hot pressing, the mesh is cooled to room temperature, and the outer edge of the cooled polyester mesh is assembled and fixed with the mesh frame to obtain a composite screen printing mesh.

9. A screen printing device, characterized in that: The invention comprises a scraper and the composite screen printing mesh as claimed in any one of claims 1 to 6.

10. A camera lens, characterized in that: It comprises a lens and an ink layer, wherein the ink layer is obtained by silk screen printing, and the silk screen printing adopts the silk screen printing device as claimed in claim 9.

Citation Information

Patent Citations

  • Composite type screen printing plate

    CN207190510U

  • Screen printing plate for solar cell printing

    CN215203974U

  • Mesh fabric for screen printing, process for preparing the same, gauze spanning method thereof and photosensitive film for screen printing plate by use thereof

    EP0439960A2

  • screen printing fabric

    FR1052526A

  • Combination screen printing plate having a plurality of extensible cushion members

    JP2000177099A