Manganese-iron atomic-scale mixed lithium manganese iron phosphate positive electrode material as well as preparation method and application thereof
The nanoscale ferromanganese hydroxide precursor is prepared by a co-precipitation method, and is sanded and calcined with a lithium source, a phosphoric acid source, and a carbon source. This solves the problem of difficult mixing of ferromanganese at the atomic level in the existing technology and achieves high-performance phosphoric acid. Preparation of lithium iron manganese cathode material with excellent electrochemical properties.
Patent Information
- Application Number
- CN202410768218.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology cannot effectively realize the lithium iron manganese phosphate cathode material mixed at the atomic level of manganese and iron, which affects the electrochemical performance of the material.
The co-precipitation method is used to mix the manganese source and the iron source according to the proportion. By adjusting the co-precipitation reaction, the nanoscale manganese ferrohydroxide precursor is obtained, and is mixed with the lithium source, phosphoric acid source, carbon source and solvent, and then sanded and sprayed for granulation. and calcination to finally prepare high-performance manganese-iron atomic-level mixed lithium iron-manganese phosphate cathode material.
Atomic-level mixing of manganese and iron is achieved, which improves the electrochemical performance of the material. The 0.1C first cycle capacity density is >150.00mAh/g, the discharge voltage is >3.90V, and the 1C discharge capacity is >137.00mAh/g.
Smart Images

Figure CN118723960A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium iron manganese phosphate (LiMn x Fe (1-x) PO4, abbreviated as LMFP) is a new type of lithium-ion battery cathode material, which has attracted widespread attention in recent years due to its unique performance and advantages. Traditional lithium-ion battery cathode materials mainly include ternary materials (NCM) and lithium iron phosphate (LFP). With the growth of electric vehicles and energy storage demand, the performance requirements for battery materials are also increasing. LMFP material combines the safety of lithium iron phosphate with the high energy density advantages of ternary materials. Compared with lithium iron phosphate, LMFP has a voltage platform of up to 4.1V, which is significantly higher than the 3.4V of lithium iron phosphate, so it can provide higher energy density. Compared with ternary materials, lithium manganese iron phosphate has higher thermal stability and lower cost. Therefore, lithium manganese iron phosphate material is expected to become one of the key materials for the next generation of high-performance lithium-ion batteries.
[0003] The preparation methods of lithium iron manganese phosphate include solid phase method and liquid phase method. The solid phase method is difficult to achieve atomic-level mixing of iron and manganese, thus affecting the electrochemical performance of the material. The liquid phase method includes hydrothermal method, sol-gel method and co-precipitation method. The hydrothermal method and sol-gel method have high requirements for equipment and are not suitable for large-scale industrialization. The co-precipitation method can achieve uniform mixing of iron and manganese, improve the capacity density of the material, and can be mass-produced. Compared with other preparation methods, the co-precipitation method is easy to make small-particle materials and improve the rate performance of the positive electrode material.
[0004] However, the coprecipitation method disclosed in the prior art still cannot obtain a lithium iron manganese phosphate positive electrode material with good manganese and iron atomic level mixing. Therefore, it is necessary to develop a new preparation method for a lithium iron manganese phosphate positive electrode material with manganese and iron atomic level mixing. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a manganese-iron atomic-level mixed manganese iron lithium phosphate positive electrode material and a preparation method and application thereof. The preparation method first adopts a coprecipitation method to mix a manganese source and an iron source according to a ratio, and obtains a nano-scale manganese iron hydroxide precursor with uniform manganese and iron mixing, small particle size and controllable ratio by adjusting the coprecipitation reaction. The precursor is used as an intermediate, mixed evenly with a lithium source, a phosphoric acid source, a carbon source and a solvent, and sand milling, spray granulation and calcination are performed in sequence to finally obtain a high-performance manganese-iron atomic-level mixed manganese iron lithium phosphate positive electrode material; the manganese-iron atomic-level mixed manganese iron lithium phosphate positive electrode material of the present invention has excellent electrochemical properties, 0.1C first cycle capacity density>150.00mAh / g, discharge voltage>3.90V, 1C discharge capacity>137.00mAh / g.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] One of the purposes of the present invention is to provide a method for preparing a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, the preparation method comprising the following steps:
[0008] The ferromanganese mixed salt solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom liquid in parallel to carry out a coprecipitation reaction, and a ferromanganese hydroxide precursor is obtained by solid-liquid separation;
[0009] The manganese iron hydroxide precursor is uniformly mixed with a lithium source, a phosphoric acid source, a carbon source and a solvent, and the obtained suspension is sequentially sand-milled, spray-granulated and calcined to obtain a manganese iron atomic-level mixed manganese iron phosphate lithium positive electrode material.
[0010] The preparation method of the present invention first adopts a co-precipitation method to mix a manganese source and an iron source according to a ratio, and obtains a nano-scale manganese iron hydroxide precursor with uniform manganese and iron mixing, small particle size and controllable ratio by adjusting the co-precipitation reaction. The precursor is used as an intermediate and is evenly mixed with a lithium source, a phosphoric acid source, a carbon source and a solvent, and sand milling, spray granulation and calcination are performed in sequence to finally obtain a high-performance manganese iron atomic-level mixed manganese iron phosphate lithium positive electrode material.
[0011] It should be noted that the reaction base solution of the present invention is prepared from pure water, a precipitant solution and a complexing agent solution, and is used to maintain the stability of the reaction system.
[0012] As a preferred technical solution of the present invention, the manganese-iron mixed salt solution includes a soluble manganese salt and a soluble ferrous salt, and the molar ratio of the two is x:(1-x); wherein, 0.6≤x≤0.9, for example, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85 or 0.9, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0013] It should be noted that the chemical formula of the ferromanganese hydroxide precursor of the present invention is Mn x Fe 1-x (OH)3, divalent iron and divalent manganese will be oxidized to trivalent ones during the solid-liquid separation process such as filtration, washing and drying.
[0014] Preferably, the soluble manganese salt comprises at least one of manganese sulfate, manganese chloride or manganese nitrate.
[0015] Preferably, the soluble ferrous salt includes at least one of ferrous sulfate, ferrous chloride or ferrous nitrate.
[0016] Preferably, the total metal salt concentration of the manganese-iron mixed salt solution is 90-110 g / L, for example 90 g / L, 95 g / L, 100 g / L, 105 g / L or 110 g / L, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0017] Preferably, the precipitant solution comprises sodium hydroxide solution or potassium hydroxide solution.
[0018] Preferably, the concentration of the precipitant solution is 9-11 mol / L, for example 9 mol / L, 9.5 mol / L, 10 mol / L, 10.5 mol / L or 11 mol / L, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0019] Preferably, the complexing agent solution includes at least one of aqueous ammonia, oxalic acid solution or EDTA solution.
[0020] Preferably, the concentration of the complexing agent solution is 7-9 mol / L, such as 7 mol / L, 7.5 mol / L, 8 mol / L, 8.5 mol / L or 9 mol / L, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0021] As a preferred technical solution of the present invention, in the parallel injection, the injection flow rate of the manganese-iron mixed salt solution is 0.3-0.5L / h, such as 0.3L / h, 0.35L / h, 0.4L / h, 0.45L / h or 0.5L / h, etc., the injection flow rate of the precipitant solution is 0.1-0.2L / h, such as 0.1L / h, 0.12L / h, 0.14L / h, 0.16L / h, 0.18L / h or 0.2L / h, etc., and the injection flow rate of the complexing agent solution is 0.08-0.12L / h, such as 0.08L / h, 0.09L / h, 0.10L / h, 0.11L / h or 0.12L / h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0022] It should be noted that, during the parallel injection process, the injection flow rates of the precipitant solution and the complexing agent solution need to be adjusted according to the required pH range and ammonia concentration range.
[0023] As a preferred technical solution of the present invention, the reaction temperature of the coprecipitation reaction is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C or 70°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0024] Preferably, the reaction pH of the coprecipitation reaction is 10.0-11.0, such as 10.0, 10.1, 10.3, 10.5, 10.7, 10.8 or 11.0, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0025] Preferably, the concentration of the complexing agent in the coprecipitation reaction is 0.5-0.6 g / L, for example 0.5 g / L, 0.51 g / L, 0.53 g / L, 0.55 g / L, 0.57 g / L, 0.58 g / L or 0.6 g / L, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0026] Preferably, the stirring speed of the coprecipitation reaction is 250-350rpm, for example, 250rpm, 270rpm, 280rpm, 300rpm, 310rpm, 330rpm or 350rpm, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0027] Preferably, the reaction time of the coprecipitation reaction is 6-7h, for example 6h, 6.1h, 6.3h, 6.5h, 6.7h, 6.8h or 7h, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0028] Preferably, the solid-liquid separation comprises filtering, washing and drying performed in sequence.
[0029] As a preferred technical solution of the present invention, the lithium source includes lithium carbonate and / or lithium hydroxide, the phosphate source includes phosphoric acid, the carbon source includes at least one of glucose, sucrose or polyvinyl alcohol, and the solvent includes deionized water.
[0030] It should be noted that the lithium source of the present invention is potassium carbonate and / or potassium hydroxide, which, compared with lithium chloride and lithium sulfate, does not introduce impurities such as chlorine and sulfur.
[0031] Preferably, the molar ratio of the ferromanganese hydroxide precursor, the lithium source, the phosphoric acid source and the carbon source is 1:(1-1.05):1:0.3.
[0032] As a preferred technical solution of the present invention, the solid content of the suspension is 40-50wt%, for example, 40wt%, 41wt%, 43wt%, 45wt%, 46wt%, 48wt% or 50wt%, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0033] Preferably, during the mixing, the stirring time is controlled to be 1-2 h, for example, 1 h, 1.1 h, 1.3 h, 1.5 h, 1.6 h, 1.8 h or 2 h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0034] As a preferred technical solution of the present invention, the sanding is carried out in a sand mill with a rotation speed of 1500-2500rpm, for example, 1500rpm, 1700rpm, 1800rpm, 2000rpm, 2100rpm, 2300rpm or 2500rpm, etc., and a time of 2-5h, for example, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, etc., but are not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0035] Preferably, the spray outlet temperature of the spray granulation is 80-150°C, for example 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0036] As a preferred technical solution of the present invention, the calcination includes a first stage calcination and a second stage calcination.
[0037] It should be noted that the calcination in the present invention is carried out in a tubular furnace, and the calcination atmosphere is controlled to be a nitrogen atmosphere.
[0038] Preferably, the heating rate of the first stage calcination is 1.5-2.5°C / min, for example, 1.5°C / min, 1.6°C / min, 1.8°C / min, 2.0°C / min, 2.1°C / min, 2.3°C / min or 2.5°C / min, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0039] Preferably, the target temperature of the first stage calcination is 300-400°C, for example, 300°C, 310°C, 330°C, 350°C, 360°C, 380°C or 400°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0040] Preferably, the calcination time is 2-5 h, such as 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0041] Preferably, the heating rate of the second-stage calcination is 1.5-2.5°C / min, for example, 1.5°C / min, 1.6°C / min, 1.8°C / min, 2°C / min, 2.1°C / min, 2.3°C / min or 2.5°C / min, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0042] Preferably, the target temperature of the second-stage calcination is 700-800°C, for example, 700°C, 710°C, 730°C, 750°C, 760°C, 780°C or 800°C, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0043] Preferably, the second-stage calcination time is 10-15 h, such as 10 h, 11 h, 12 h, 13 h, 14 h or 15 h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0044] The second object of the present invention is to provide a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, which is prepared by the preparation method described in the first object.
[0045] The third object of the present invention is to provide an application of a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, and to apply the manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material to the preparation of a lithium-ion battery;
[0046] Among them, the manganese-iron atomic-level mixed manganese iron lithium phosphate positive electrode material is prepared by the preparation method described in purpose one, or the manganese-iron atomic-level mixed manganese iron lithium phosphate positive electrode material is the manganese-iron atomic-level mixed manganese iron lithium phosphate positive electrode material described in purpose two.
[0047] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0048] (1) The preparation method of the present invention prepares Fe by coprecipitation x Mn 1-x (OH)3 precursor can achieve atomic-level mixing of iron and manganese, and simultaneously synthesize small-sized Fe x Mn 1-x (OH)3 precursor is conducive to the subsequent sand grinding to prepare lithium manganese iron phosphate positive electrode materials with smaller particle size and provide higher rate performance;
[0049] (2) The preparation method of the present invention is based on Fe x Mn 1-x The lithium manganese iron phosphate positive electrode material prepared using (OH)3 precursor as intermediate exhibits high discharge voltage and rate performance, with 0.1C first cycle capacity density >150.00mAh / g, discharge voltage >3.90V, and 1C discharge capacity >137.00mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 is a SEM image of the ferromanganese hydroxide precursor prepared in Example 1 of the present invention;
[0051] Figure 2 This is an EDS image of the ferromanganese hydroxide precursor prepared in Example 1 of the present invention for the Mn element;
[0052] Figure 3 This is an EDS image of the ferromanganese hydroxide precursor prepared in Example 1 of the present invention for the Fe element;
[0053] Figure 4 This is a SEM image of the manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material obtained in Example 1 of the present invention;
[0054] Figure 5 This is a charge and discharge curve diagram of the manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0055] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0056] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0057] Example 1
[0058] This embodiment provides a method for preparing a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, the preparation method comprising the following steps:
[0059] Dissolve manganese sulfate and ferrous sulfate in water at a molar ratio of Mn:Fe=0.6:0.4 to prepare a 100 g / L manganese-iron mixed salt solution;
[0060] In a reaction kettle, a reaction base liquid is prepared by preparing pure water, a precipitant solution and a complexing agent solution. In a nitrogen atmosphere, the manganese-iron mixed salt solution, a 10 mol / L sodium hydroxide solution and an 8 mol / L ammonia water are injected into the reaction base liquid in parallel to carry out a coprecipitation reaction. The reaction temperature is controlled to be 60° C., the reaction pH is 10.5, the ammonia concentration is 0.55 g / L, the stirring speed is 300 rpm, and after stirring for 7 hours, filtering, washing and drying are carried out in sequence to obtain a product with a chemical formula of Mn 0.6 Fe 0.4 (OH)3 manganese ferrohydroxide precursor;
[0061] Figure 1 The SEM image of the obtained ferromanganese hydroxide precursor is shown. It can be seen that the ferromanganese hydroxide precursor prepared in this embodiment has a nanoscale flake morphology; Figure 2 and Figure 3 The EDS images of the obtained manganese ferrohydroxide precursor for the Mn element and the Fe element are shown respectively, and it can be seen that the Mn element and the Fe element are evenly distributed, and the manganese and iron atoms are mixed;
[0062] The manganese iron hydroxide precursor is mixed with lithium carbonate, phosphoric acid and glucose in a ratio of 1:1.02:1:0.3 and dissolved in deionized water with a solid content of 45wt%. After stirring for 1 hour, the obtained suspension is poured into a sand mill for sand grinding. The sand mill speed is set to 2000rpm and the sand milling time is 3 hours. The suspension after sand grinding is spray granulated and the spray outlet temperature is adjusted to 100°C. The dried material after spraying is collected and loaded into a porcelain boat, and calcined in a nitrogen atmosphere of a tubular furnace. The temperature is first increased to 350°C at 2°C / min and maintained for 3 hours for a first calcination, and then increased to 750°C at 2°C / min and maintained for 10 hours for a second calcination. The manganese iron atomic-level mixed manganese iron phosphate lithium positive electrode material is naturally cooled to obtain a chemical formula of LiMn 0.6 Fe 0.4 PO4.
[0063] Figure 4 The SEM image of the obtained manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material is shown, and it can be seen that the particle size of the manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material is at the nanometer level, and the particle size distribution is relatively uniform.
[0064] Example 2
[0065] This embodiment provides a method for preparing a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, the preparation method comprising the following steps:
[0066] Dissolve manganese sulfate and ferrous sulfate in water at a molar ratio of Mn:Fe=0.6:0.4 to prepare a 90 g / L manganese-iron mixed salt solution;
[0067] In a reaction kettle, a reaction base liquid is prepared by preparing pure water, a precipitant solution and a complexing agent solution. In a nitrogen atmosphere, the manganese-iron mixed salt solution, a 9 mol / L sodium hydroxide solution and a 7 mol / L ammonia water are injected into the reaction base liquid in parallel, the injection flow rate of the manganese-iron mixed salt solution is 0.3 L / h, the injection flow rate of the precipitant solution is 0.1 L / h, and the injection flow rate of the complexing agent solution is 0.08 L / h. A coprecipitation reaction is carried out, and the reaction temperature is controlled to be 50° C., the reaction pH is 10.0, the ammonia concentration is 0.5 g / L, the stirring speed is 250 rpm, and after stirring for 6 hours, filtering, washing and drying are carried out in sequence to obtain a chemical formula of Mn 0.6 Fe 0.4 (OH)3 manganese ferrohydroxide precursor;
[0068] The manganese iron hydroxide precursor is mixed with lithium carbonate, phosphoric acid and glucose in a ratio of 1:1.02:1:0.3 and dissolved in deionized water with a solid content of 40wt%. After stirring for 1 hour, the obtained suspension is poured into a sand mill for sand grinding. The sand mill speed is set to 1500rpm and the sand milling time is 2 hours. The suspension after sand grinding is spray granulated and the spray outlet temperature is adjusted to 80°C. The dried material after spraying is collected and loaded into a porcelain boat, and calcined in a nitrogen atmosphere of a tubular furnace. The temperature is first increased to 300°C at 1.5°C / min and maintained for 2 hours for a first calcination, and then increased to 700°C at 1.5°C / min and maintained for 10 hours for a second calcination. The manganese iron atomic level mixed manganese iron phosphate lithium positive electrode material is naturally cooled to obtain a chemical formula of LiMn 0.6 Fe 0.4 PO4.
[0069] Example 3
[0070] This embodiment provides a method for preparing a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, the preparation method comprising the following steps:
[0071] Dissolve manganese sulfate and ferrous sulfate in water at a molar ratio of Mn:Fe=0.6:0.4 to prepare a 110 g / L manganese-iron mixed salt solution;
[0072] In a reaction kettle, a reaction base liquid is prepared by preparing pure water, a precipitant solution and a complexing agent solution. In a nitrogen atmosphere, the manganese-iron mixed salt solution, an 11 mol / L sodium hydroxide solution and a 9 mol / L ammonia water are injected into the reaction base liquid in parallel, the injection flow rate of the manganese-iron mixed salt solution is 0.5 L / h, the injection flow rate of the precipitant solution is 0.2 L / h, and the injection flow rate of the complexing agent solution is 0.12 L / h. A coprecipitation reaction is carried out, the reaction temperature is controlled to be 70° C., the reaction pH is 11.0, the ammonia concentration is 0.6 g / L, the stirring speed is 350 rpm, and after stirring for 7 hours, filtering, washing and drying are carried out in sequence to obtain a chemical formula of Mn0.6 Fe 0.4 (OH)3 manganese ferrohydroxide precursor;
[0073] The ferromanganese hydroxide precursor is mixed with lithium carbonate, phosphoric acid and glucose in a ratio of 1:1.02:1:0.3 and dissolved in deionized water with a solid content of 50wt%. After stirring for 2h, the obtained suspension is poured into a sand mill for sand milling. The sand milling speed is set to 2500rpm and the sand milling time is 5h. The suspension after sand milling is spray granulated and the spray outlet temperature is adjusted to 150°C. The dried material after spraying is collected and loaded into a porcelain boat, and calcined in a nitrogen atmosphere of a tubular furnace. The temperature is first increased to 400°C at 2.5°C / min and maintained for 5h for a first-stage calcination, and then increased to 800°C at 2.5°C / min and maintained for 15h for a second-stage calcination. The manganese iron atomic-level mixed manganese iron phosphate lithium positive electrode material is naturally cooled to obtain a chemical formula of LiMn 0.6 Fe 0.4 PO4.
[0074] Comparative Example 1
[0075] This comparative example provides a method for preparing a lithium manganese iron phosphate positive electrode material, the preparation method comprising the following steps:
[0076] Manganese sulfate, ferrous sulfate, lithium carbonate, phosphoric acid, and glucose were mixed and dissolved in deionized water at a ratio of 0.6:0.4:1.02:1:0.3. After stirring for 1 hour, the solid content was 40wt%. The obtained suspension was poured into a sand mill for sand milling. The sand milling speed was set to 2000rpm and the sand milling time was 3 hours. The suspension after sand milling was spray granulated and the spray outlet temperature was adjusted to 100°C. The dried material after spraying was collected and loaded into a porcelain boat, and calcined in a nitrogen atmosphere of a tubular furnace. The temperature was first increased to 350°C at 2°C / min and maintained for 3 hours for a first-stage calcination, and then increased to 750°C at 2°C / min and maintained for 10 hours for a second-stage calcination. The lithium iron manganese phosphate positive electrode material was naturally cooled and the chemical formula was LiMn 0.6 Fe 0.4 PO4.
[0077] The lithium iron manganese phosphate positive electrode material obtained in the above examples and comparative examples was made into a positive electrode plate of a lithium ion battery, a metal lithium plate was used as a negative electrode plate, a polyethylene film was used as a separator, and lithium hexafluorophosphate was used as an electrolyte to assemble into a button battery, and then the charge and discharge conditions of the first cycle of 0.1C, 0.2C, 0.5C, and 1C were measured, and the discharge voltage and rate performance of the positive electrode material were detected. The specific results of the 0.1C first cycle capacity density, discharge voltage, and 1C discharge capacity are summarized in Table 1; wherein, Figure 5The charge and discharge curves of the manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material obtained in Example 1 are shown. It can be seen that the obtained positive electrode material has high discharge voltage and rate performance, with a 0.1C first cycle capacity density of 156.91 mAh / g, a discharge voltage of 3.94 V, and a 1C discharge capacity of 140.10 mAh / g.
[0078] Table 1
[0079] project 0.1C first cycle capacity density (mAh / g) Discharge voltage(V) 1C discharge capacity (mAh / g) Example 1 156.91 3.94 140.10 Example 2 150.10 3.93 138.01 Example 3 150.36 3.93 137.75 Comparative Example 1 145.86 3.92 135.54
[0080] In summary, the present invention provides a manganese-iron atomic-level mixed manganese iron lithium iron phosphate positive electrode material and a preparation method and application thereof. The preparation method first adopts a coprecipitation method to mix a manganese source and an iron source according to a ratio, and obtains a nano-scale manganese iron hydroxide precursor with uniform manganese and iron mixing, small particle size and controllable ratio by adjusting the coprecipitation reaction. The precursor is used as an intermediate, mixed evenly with a lithium source, a phosphoric acid source, a carbon source and a solvent, and sand milling, spray granulation and calcination are performed in sequence to finally obtain a high-performance manganese-iron atomic-level mixed manganese iron lithium iron phosphate positive electrode material; the manganese-iron atomic-level mixed manganese iron lithium iron phosphate positive electrode material of the present invention has excellent electrochemical properties, 0.1C first cycle capacity density>150.00mAh / g, discharge voltage>3.90V, 1C discharge capacity>137.00mAh / g.
[0081] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0082] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0083] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0084] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, It is characterized in that The preparation method comprises the following steps: The ferromanganese mixed salt solution, the precipitant solution and the complexing agent solution are injected into the reaction bottom liquid in parallel to carry out a coprecipitation reaction, and a ferromanganese hydroxide precursor is obtained by solid-liquid separation; The manganese iron hydroxide precursor is uniformly mixed with a lithium source, a phosphoric acid source, a carbon source and a solvent, and the obtained suspension is sequentially sand-milled, spray-granulated and calcined to obtain a manganese iron atomic-level mixed manganese iron phosphate lithium positive electrode material.
2. The preparation method according to claim 1, It is characterized in that The manganese-iron mixed salt solution includes a soluble manganese salt and a soluble ferrous salt, and the molar ratio of the two is x:(1-x); wherein 0.6≤x≤0.9; Preferably, the soluble manganese salt comprises at least one of manganese sulfate, manganese chloride or manganese nitrate; Preferably, the soluble ferrous salt comprises at least one of ferrous sulfate, ferrous chloride or ferrous nitrate; Preferably, the total metal salt concentration of the manganese-iron mixed salt solution is 90-110 g / L; Preferably, the precipitant solution comprises sodium hydroxide solution or potassium hydroxide solution; Preferably, the concentration of the precipitant solution is 9-11 mol / L; Preferably, the complexing agent solution includes at least one of ammonia solution, oxalic acid solution or EDTA solution; Preferably, the concentration of the complexing agent solution is 7-9 mol / L.
3. The preparation method according to claim 1 or 2, It is characterized in that In the parallel flow injection, the injection flow rate of the manganese-iron mixed salt solution is 0.3-0.5 L / h, the injection flow rate of the precipitant solution is 0.1-0.2 L / h, and the injection flow rate of the complexing agent solution is 0.08-0.12 L / h.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The reaction temperature of the coprecipitation reaction is 50-70°C; Preferably, the reaction pH of the coprecipitation reaction is 10.0-11.0; Preferably, the concentration of the complexing agent in the coprecipitation reaction is 0.5-0.6 g / L; Preferably, the stirring speed of the coprecipitation reaction is 250-350 rpm; Preferably, the reaction time of the coprecipitation reaction is 6-7h; Preferably, the solid-liquid separation comprises filtering, washing and drying performed in sequence.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The lithium source comprises lithium carbonate and / or lithium hydroxide, the phosphoric acid source comprises phosphoric acid, the carbon source comprises at least one of glucose, sucrose or polyvinyl alcohol, and the solvent comprises deionized water; Preferably, the molar ratio of the ferromanganese hydroxide precursor, the lithium source, the phosphoric acid source and the carbon source is 1:(1-1.05):1:0.
3.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The solid content of the suspension is 40-50wt%; Preferably, during the mixing, the stirring time is controlled to be 1-2 hours.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The sand grinding is carried out in a sand mill at a rotation speed of 1500-2500 rpm for 2-5 hours; Preferably, the spray outlet temperature of the spray granulation is 80-150°C.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The calcination includes a first stage calcination and a second stage calcination; Preferably, the heating rate of the first stage calcination is 1.5-2.5°C / min; Preferably, the target temperature of the first stage calcination is 300-400°C; Preferably, the calcination period is 2-5 hours; Preferably, the heating rate of the second-stage calcination is 1.5-2.5°C / min; Preferably, the target temperature of the second stage calcination is 700-800°C; Preferably, the second-stage calcination time is 10-15 hours.
9. A manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, It is characterized in that The preparation method is described in any one of claims 1 to 8.
10. Application of a manganese-iron atomic-level mixed manganese iron phosphate lithium positive electrode material, It is characterized in that Applying manganese iron atomic-level mixed manganese iron phosphate lithium positive electrode material to the preparation of lithium-ion batteries; The manganese-iron atomic-level mixed manganese iron lithium iron phosphate positive electrode material is prepared by the preparation method described in any one of claims 1 to 8, or the manganese-iron atomic-level mixed manganese iron lithium iron phosphate positive electrode material is the manganese-iron atomic-level mixed manganese iron lithium iron phosphate positive electrode material described in claim 9.
Citation Information
Patent Citations
Olivine type positive electrode material as well as preparation method and application thereof
CN117996071A
Cited By
Preparation method of lithium-rich manganese-based positive electrode material
CN118954633A
A method for preparing lithium-rich manganese-based positive electrode material
CN118954633B
Lithium manganese iron phosphate precursor and preparation method of lithium manganese iron phosphate
CN119284859A
Dual-coated ternary positive electrode material as well as preparation method and application thereof
CN119852377A
Ferromanganese phosphate precursor, lithium iron manganese phosphate, preparation method of lithium iron manganese phosphate, battery monomer, battery device and power utilization device
CN120039853A