Method for preparing rare earth hexaboride nanometer material through molten salt method

By ball milling and calcining rare earth hexaboride at low temperature by melting salt method, the problems of high temperature, high cost and large particle size in the existing process are solved, and the low cost and high activity preparation of rare earth hexaboride nanomaterials are realized, suitable for photothermal Catalytic field.

CN118978168APending Publication Date: 2024-11-19SHAOXING INST OF NEW ENERGY & MOLECULAR ENG SHANGHAI JIAO TONG UNIV

Patent Information

Application Number
CN202411061425.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing lanthanum hexaboride preparation process requires high reaction temperature, high equipment requirements, complex process, high production cost, and large particle size and weak local plasma surface resonance effect, which limits its photothermal catalysis. Application in the field.

Method used

Rare earth hexaboride nanomaterials were prepared by molten salt method, and the rare earth hexaboride nanomaterials were synthesized at low temperature by ball milling in zirconia ball grinding medium and calcining in an argon atmosphere.

Benefits of technology

It realizes low temperature synthesis, reduces energy consumption, low production cost, and has small particle size, high activity and simple process, which is suitable for photothermal catalyst support.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978168A_ABST
    Figure CN118978168A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a rare earth hexaboride nano-material by a molten salt method, and relates to the technical field of material preparation, and the method comprises the following steps: (1) weighing a rare earth precursor, a boron precursor and molten salt in sequence according to a certain stoichiometric ratio, taking a zirconium oxide ball as a grinding medium, and then placing in a grinding tank; (2) putting the ball milling tank filled with the sample into a planetary ball mill for ball milling; (3) putting the ball-milled product into a tubular furnace, and calcining in an argon atmosphere; and (4) washing, centrifuging and drying the calcined sample to obtain the rare earth hexaboride nano material LnB6. The hexaboride synthesized by the method is small in particle size and high in activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation, and in particular to a method for preparing rare earth hexaboride nanomaterials by a molten salt method. Background Art

[0002] Hexaboride, represented by lanthanum hexaboride, is an excellent electron emitter material with high melting point, high conductivity, high stability, and low work function. These excellent properties have led to the wide application of lanthanum hexaboride in electronic devices such as electron microscopes, free electron lasers, and vacuum electron beams. In recent years, studies have found that LaB6 has a strong localized surface plasmon resonance effect near 1000nm. This effect enables LaB6 nanoparticles to effectively absorb near-infrared light in sunlight, converting light energy into heat energy to realize the development and utilization of solar energy. This feature also makes LaB6 show broad application prospects in the field of photothermal catalysis.

[0003] As the application field of LaB6 continues to expand, research on the preparation process of LaB6 is also deepening. So far, many methods for synthesizing LaB6 have been developed, such as the pressing or spark plasma sintering method for making bulk LaB6, the chemical vapor deposition method for preparing LaB6 nanowires, and the carbon thermal reduction method for preparing micron-sized LaB6 powder. However, these methods often require extremely high reaction temperatures, high equipment requirements, complex preparation processes, high production costs, and the resulting particles are large in size and the localized plasma surface resonance effect is weak, which limits its application in the field of photothermal catalysis. Therefore, the development of a new and effective preparation technology for preparing small-sized LaB6 nanoparticles is the key to solving these process problems. Summary of the invention

[0004] In view of a series of problems existing in the existing preparation process, the present invention provides a method for preparing rare earth hexaboride nanomaterials (LnB6) by a molten salt method, which is of great significance for the later development of highly active LnB6 photothermal catalysts.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A method for preparing rare earth hexaboride nanomaterials by a molten salt method comprises the following steps:

[0007] (1) weighing a rare earth precursor, a boron precursor and a molten salt in sequence according to a certain stoichiometric ratio, using zirconium oxide balls as grinding media, and then placing them in a grinding jar;

[0008] (2) placing the ball mill jar filled with the sample in a planetary ball mill for ball milling;

[0009] (3) placing the ball-milled product in a tube furnace and calcining it in an argon atmosphere;

[0010] (4) The calcined sample is washed, centrifuged and dried to obtain rare earth hexaboride nanomaterial LnB6.

[0011] Further settings are as follows:

[0012] In step (1):

[0013] The rare earth elements contained in the rare earth precursor include but are not limited to La, Ce, Pr, Nd, Sm or Eu.

[0014] The rare earth precursor is preferably a rare earth chloride.

[0015] The boron precursor is a borohydride salt, preferably any one or more of sodium borohydride, potassium borohydride, and lithium borohydride.

[0016] The molten salt is one or more of LiCl, KCl, and NaCl.

[0017] In the reactants, the molar ratio of rare earth chloride to borohydride is 1:5-10, preferably 1:6.

[0018] The reactants include rare earth chloride and borohydride, and the mass ratio of the reactants to the molten salt is 1:5-10, preferably 1:10.

[0019] The grinding medium is a zirconia ball with a diameter of 5-10 mm.

[0020] The ball-to-material mass ratio, i.e., the mass ratio of the zirconia ball to the material, is preferably 5-10:1.

[0021] In step (2):

[0022] The ball milling is carried out under a protective atmosphere, which is argon.

[0023] The ball milling speed is 300-600 r / min, and the ball milling time is 0-5 h.

[0024] In step (3):

[0025] The calcination temperature is 360-800° C., and the calcination time is 3-12 hours.

[0026] The second aspect of the present invention is to provide an application of the LnB6 nanomaterial prepared above in a catalyst carrier for photothermal ammonia synthesis reaction.

[0027] The method of the present invention has the following beneficial effects:

[0028] 1. The raw materials are cheap and easy to obtain, which greatly reduces the production cost.

[0029] 2. Realize low-temperature synthesis of LnB6 and reduce energy consumption.

[0030] 3. The synthesized hexaboride has small particle size and high activity.

[0031] 4. Simple process and easy operation.

[0032] The following is a further description of the implementation scheme of the present invention in conjunction with the accompanying drawings. The following examples are implemented on the premise of the scheme of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the above-mentioned examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the XRD pattern of LaB6 prepared in Example 1.

[0034] Figure 2 TEM image of LaB6 prepared in Example 1.

[0035] Figure 3 This is the UV-vis spectrum of LaB6 prepared in Example 1.

[0036] Figure 4 XRD patterns of other LnB6 nanomaterials prepared in Examples 5-9. DETAILED DESCRIPTION

[0037] Example 1

[0038] (1) LaCl3 and NaBH4 were weighed as reactants at a molar ratio of lanthanum atoms to boron atoms of 1:6, and molten salts LiCl and KCl were weighed at a mass ratio of reactants to molten salt of 1:10, with the mass ratio of LiCl to KCl in the molten salt being 45:55. The reactants were then placed in a 250 mL grinding jar, and zirconia balls were used as grinding media. The diameters of the zirconia balls were selected to be 5, 8, and 10 mm, and the mass ratio was 5:3:2. The mass ratio of the zirconia balls to the material was controlled to be 10:1.

[0039] (2) The ball mill jar filled with the sample was placed in a planetary ball mill for ball milling in a high-purity Ar atmosphere. The speed of the ball mill was 400 r / min, the ball milling time was set to 2.5 h, and sampling was performed.

[0040] (3) The ball-milled product was transferred to a tubular furnace and calcined at 600 °C for 3 h in an argon atmosphere.

[0041] (4) The calcined sample is washed with water and ethanol and centrifuged multiple times. After the last centrifugation, the sample is placed in an oven for drying at 70°C for 8 hours to obtain LaB6 nanomaterials.

[0042] Product Confirmation:

[0043] like Figure 1-Figure 3 As shown: the LaB6 obtained in Example 1 is consistent with the standard card and has no impurities, proving the feasibility of the low-temperature molten salt method in the synthesis of LnB6. The particle size of the obtained LaB6 is small and the size distribution is uniform, about 30nm. And LaB6 shows strong absorption in the ultraviolet and near-infrared regions, corresponding to the localized surface plasmon resonance (LSPR) effect of LaB6.

[0044] Example 2

[0045] The preparation method is the same as that in Example 1, except that in step (1), the mass ratio of zirconium oxide balls to the material is controlled to be 5:1, and a nano-LaB6 material with a particle size of 42 nm is prepared.

[0046] Example 3

[0047] The preparation method is the same as that of Example 1, except that in step (1), the mass ratio of the reactant to the molten salt is adjusted to 1:5, and a nano-LaB6 material with a particle size of 60 nm is prepared.

[0048] Example 4

[0049] The preparation method is the same as that in Example 1, except that in step (2), the rotation speed of the ball mill is adjusted to 600 r / min, and the ball milling time is set to 3 h, so as to prepare a nano-LaB6 material with a particle size of 25 nm.

[0050] Combined with the examples 2-4, in the preparation method involved in this patent, the particle size of the obtained hexaboride nanoparticles can be adjusted by adjusting the preparation process. Specifically, according to the comparison between Examples 1 and 2, increasing the mass ratio of zirconium oxide balls to reactant materials can reduce the particle size of LnB6, and adjusting from 10:1 to 5:1, the obtained LnB6 particles become larger; according to the comparison between Examples 1 and 3, increasing the proportion of molten salt in the feed can reduce the particle size of LnB6; according to the comparison between Examples 1 and 4, increasing the speed of the ball mill can make the prepared particle size smaller.

[0051] Example 5

[0052] The preparation method is the same as that of Example 1, except that in step (1), the rare earth chloride is replaced with CeCl3 to prepare CeB6 nanomaterial.

[0053] Example 6

[0054] The preparation method is the same as that of Example 1, except that in step (1), the rare earth chloride is replaced with PrCl3 to prepare PrB6 nanomaterial.

[0055] Example 7

[0056] The preparation method is the same as that in Example 1, except that in step (1), the rare earth chloride is replaced with NdCl3 to prepare nano-NdB6 material.

[0057] Example 8

[0058] The preparation method is the same as that in Example 1, except that in step (1), the rare earth chloride is replaced with SmCl3 to prepare SmB6 nanomaterial.

[0059] Example 9

[0060] The preparation method is the same as that of Example 1, except that in step (1), the rare earth chloride is changed to EuCl3, thereby obtaining EuB6 nanomaterials.

[0061] The XRD patterns of the nanomaterials prepared in Examples 5-9 are as follows: Figure 4 As shown, according to the attached Figure 4 The provided XRD shows that the molten salt method proposed in this patent can be used to successfully prepare a variety of rare earth hexaborides LnB6 at low temperatures, including but not limited to LaB6, CeB6, PrB6, NdB6, SmB6, and EuB6. This preparation method has a certain universality and can be extended to other hexaboride systems.

[0062] Application examples:

[0063] The LaB6 nanomaterial prepared in Example 1 was used as a catalyst support for the photothermal ammonia synthesis reaction, and its photothermal ammonia synthesis activity was tested.

[0064] The experimental method is as follows:

[0065] Take 90mg LaB6 and 21mg Ru3(CO) 12 After grinding, the temperature was raised to 250°C at a heating rate of 0.5° / min in a tube furnace in a H2 / Ar atmosphere, maintained at 250°C for 2 hours, and then naturally cooled to room temperature to obtain a catalyst.

[0066] 100 mg of the obtained catalyst was loaded onto a fixed bed, the flow rates of N2 and H2 were set to 15 mL / min and 45 mL / min, respectively, and a xenon lamp was turned on to test the activity of the catalyst in photothermal synthesis of ammonia under illumination.

[0067] The experimental results are as follows:

[0068] The photothermal activity of the catalyst Ru-LaB6 under light irradiation was tested to be 405 μmol g -1 h -1 , which is three times that in dark conditions.

Claims

1. A method for preparing rare earth hexaboride nanomaterials by a molten salt method, characterized in that: The following steps are involved: (1) weighing a rare earth precursor, a boron precursor and a molten salt in sequence according to a certain stoichiometric ratio, using zirconium oxide balls as grinding media, and then placing them in a grinding jar; (2) placing the ball mill jar filled with the sample in a planetary ball mill for ball milling; (3) placing the ball-milled product in a tube furnace and calcining it in an argon atmosphere; (4) The calcined sample is washed, centrifuged and dried to obtain rare earth hexaboride nanomaterial LnB6.

2. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (1): the rare earth elements contained in the rare earth precursor include but are not limited to La, Ce, Pr, Nd, Sm or Eu.

3. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (1): the rare earth precursor is a rare earth chloride.

4. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (1): the boron precursor is a borohydride salt selected from any one or more of sodium borohydride, potassium borohydride, and lithium borohydride.

5. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (1): the molten salt is one or more of LiCl, KCl, and NaCl.

6. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (1): in the reactants, the molar ratio of rare earth chloride to borohydride is 1:5-10, and the mass ratio of the reactants to the molten salt is 1:5-10.

7. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (1), the grinding medium is a zirconia ball with a diameter of 5-10 mm, and the mass ratio of the zirconia ball to the material is 5-10:

1.

8. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (2): the ball milling is carried out under a protective atmosphere, the protective atmosphere is argon, the ball milling speed is 300-600 r / min, and the ball milling time is 0-5 h.

9. The method for preparing rare earth hexaboride nanomaterials by a molten salt method according to claim 1, characterized in that: In step (3): the calcination temperature is 360-800°C, and the calcination time is 3-12h.

10. Use of a rare earth hexaboride nanomaterial prepared by the method of any one of claims 1 to 9 as a catalyst carrier for photothermal ammonia synthesis reaction.

Citation Information

Patent Citations

  • Preparation method of lanthanum hexaboride nanometer powder and application of lanthanum hexaboride nanometer powder

    CN106395843A

  • General synthesis of metal borides in liquid salt melts

    EP2423164A1

Cited By

  • Rare earth boride nanometer material and preparation method and application thereof

    CN120117616A

  • Pd-loaded photo-thermal catalyst as well as preparation method and application thereof

    CN120618466A

  • A pd-loaded photothermal catalyst, a preparation method and application thereof

    CN120618466B