Process for preparing zinc oxide from DMAC cuprous bromide hazardous waste and application

The process of preparing zinc oxide from DMAC cuprous bromide hazardous waste solves the problem of treatment and recycling of cuprous bromide hazardous waste, realizes the preparation of high-purity zinc oxide and the recovery of catalytic metals, and improves the utilization rate of raw materials and technology Efficient, suitable for treating organic solvent systems containing catalytic metal halide compounds.

CN118724048APending Publication Date: 2024-10-01ZHEJIANG HONGDIAN ENVIRONMENTAL PROTECTION EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410946161.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technologies fail to effectively process and recycle cuprous bromide hazardous waste, especially considering the lack of effective methods for the recovery of copper and bromine. Traditional treatment methods are inefficient and may pollute the environment.

Method used

The process of preparing zinc oxide using DMAC cuprous bromide hazardous waste includes preliminary sorting, grinding and pretreatment, reduction reaction, separation and purification, sodium bromide solution pretreatment and electrolysis, zinc oxide recovery and calcination, etc., through Zinc powder reducing agent and high-temperature calcination and other processes realize the preparation of high-purity zinc oxide.

Benefits of technology

It improves the utilization rate of raw materials, realizes the recovery of reducing agent zinc powder, and prepares high-purity zinc oxide powder with a zinc oxide purity greater than 99.9%. It simplifies the process flow, improves product purity, and is suitable for treating catalytic metal halogen systems. Compounds in organic solvent systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724048A_ABST
    Figure CN118724048A_ABST
Patent Text Reader

Abstract

The invention discloses a process for preparing zinc oxide by using DMAC cuprous bromide hazardous waste and application. According to the technology, the cuprous bromide hazardous waste is used for preparing the superfine copper powder and the sodium bromide, meanwhile, the added reducing agent zinc powder and other reducing metal are recycled, and the high-purity zinc oxide powder is prepared. Through sodium carbonate precipitation, high-temperature calcination and other processes, the purity of zinc oxide is greater than 99.9%, compared with the same type of processes, the high-temperature calcination and one-time ammonia distillation process is adopted, the operation flow is short, the process is relatively simple, and the product purity is high. The method provided by the invention not only improves the utilization rate of the raw materials, but also realizes efficient recovery of each substance, has good application prospect and popularization value, and is suitable for treating an organic solvent system containing catalytic metal halide compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hazardous waste treatment, and specifically relates to a production process for preparing zinc oxide by utilizing DMAC (dimethylacetamide) cuprous bromide hazardous waste, and application of the production process. Background Art

[0002] In the context of industrial development, the generation and treatment of cuprous bromide hazardous waste has become an urgent issue. Cuprous bromide hazardous waste mainly comes from waste catalysts in organic synthesis reactions, which are widely used in alkylation reactions of brominated acyl chlorides, coupling nitrogen reactions, and photosensitizer components in the photographic industry. In addition, cuprous bromide is also used in catalytic reactions in other organic chemistry research.

[0003] Traditional methods for treating cuprous bromide hazardous waste include landfill and incineration, but these methods are inefficient and may cause secondary pollution to the environment. Specifically:

[0004] 1. Landfill method: It involves the safe landfill of cuprous bromide hazardous waste. It is necessary to select a suitable site and follow relevant standards for design and construction to reduce the impact on the environment.

[0005] 2. Incineration method: Through high-temperature decomposition and deep oxidation processes, cuprous bromide hazardous waste is converted into harmless substances, reducing the waste volume and removing toxicity, but attention should be paid to the treatment of waste gas and waste residue generated by incineration.

[0006] 3. Chemical method: Use chemical reactions to convert cuprous bromide hazardous waste into harmless end products, such as through acid-base neutralization, oxidation-reduction or precipitation.

[0007] 4. Recycling: Consider using appropriate technologies to recover valuable components from cuprous bromide hazardous waste to achieve resource recycling.

[0008] At present, there are no specific cases of cuprous bromide hazardous waste recycling in China, but scientific research institutions and environmental protection companies are researching and developing related technologies. Existing literature provides different methods for preparing copper powder, but does not consider the impact of other organic matter on copper powder, and does not achieve the recovery of bromine. Therefore, it is of great practical significance to develop an environmentally friendly and efficient method for treating cuprous bromide hazardous waste. Summary of the invention

[0009] In view of the above-mentioned shortcomings and deficiencies in the existing cuprous bromide hazardous waste recycling and treatment, the present invention provides a process for preparing zinc oxide using DMAC cuprous bromide hazardous waste.

[0010] The present invention uses DMAC cuprous bromide hazardous waste to prepare zinc oxide, which specifically includes the following steps:

[0011] Step 1: Raw material preparation

[0012] Collect cuprous bromide hazardous waste (derived from but not limited to the residue produced by falling film evaporation of the filtrate after neutralization and precipitation filtration in the tetrafluorobutadiene production process after zincation, the copper content in the hazardous waste is about 15%, mainly in the form of cuprous (I) precipitation, and a small part in the form of copper (II), and the hazardous waste contains about 35% DMAC, so the hazardous waste is partially dissolved in water, but the aqueous solution still exists in the form of solid precipitation), and perform preliminary sorting on it to remove impurities and pollutants;

[0013] Step 2: Grinding and pretreatment

[0014] The cuprous bromide hazardous waste is ground and sieved, and then cleaned with 2-16% methanol-containing ethyl acetate cleaning solution; the ratio of hazardous waste to cleaning solution is 1:1-1:3, and the cleaning time is 30-150 minutes; after cleaning, the solid is stored for use in subsequent processes;

[0015] Step 3: Reduction reaction

[0016] Add the pretreated cuprous bromide hazardous waste solids into the reaction tank, disperse them in water at a ratio of 1:1, add the reducing agent after stirring for reaction, and the stirring speed is 200~1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80~90℃, and the reaction time is 1~8h; during the reaction, spray isomeric tridecanol, propylene glycol, n-butanol or phenylethanol dispersant (first, to make the copper powder production process uniform and control the particle size at the micron level, and second, to play a defoaming role);

[0017] Step 4: Separation and purification

[0018] After the reduction reaction is completed, the reaction product is separated from the unreacted substance by filtering or centrifugation, and the obtained solid is a crude ultrafine copper powder, and the liquid is a solution containing sodium bromide;

[0019] Step 5: Sodium bromide solution pretreatment and electrolysis

[0020] Pre-treating the sodium bromide solution by dichloromethane extraction or sodium hypochlorite oxidation to remove most of the residual organic matter; and electrolyzing to prepare bromine;

[0021] Step 6: Recovery of zinc oxide

[0022] In step 5, a sodium carbonate solution is added to the waste liquid after electrolysis to precipitate zinc ions, and the solid is separated by filtration; zinc oxide is prepared by high-temperature calcination, and organic matter in the solid is calcined at the same time; the calcined zinc oxide is purified by ammonia water, and the zinc oxide is purified by an ammonia evaporation process;

[0023] Step 7: Product Testing

[0024] The prepared zinc oxide is subjected to quality inspection to ensure that the product meets relevant standards.

[0025] On the basis of the above technical solution, the present invention optimizes and defines the nodes and steps of the preparation process, specifically including the following three aspects:

[0026] 1. In the grinding and pretreatment of step 2, it is preferred to use 8% methanol-containing ethyl acetate cleaning solution to clean the cuprous bromide hazardous waste, the ratio of hazardous waste to cleaning solution is preferably 1:1~1:1.5, and the cleaning time is preferably 120 min.

[0027] 2. In the reduction reaction of step 3, zinc powder is used as the reducing agent; the stirring speed is preferably 1400-1600 rps; the reaction time is preferably 4 h; and 1-3% of isotridecyl alcohol is sprayed during the reaction.

[0028] 3. In the recovery of zinc oxide in step 6, the calcination temperature is preferably 300-450°C; the ratio of the amount of ammonia water added to zinc oxide is preferably 10:1; and the temperature of the ammonia evaporation process is preferably 95-105°C.

[0029] In addition, the present invention also provides the application of the zinc oxide preparation: application in an organic solvent system of a halogen compound containing a catalytic metal; the catalytic metal includes nickel, copper, silver, gold, platinum or palladium.

[0030] Beneficial effects of the present invention:

[0031] The present invention uses an innovative process to prepare ultrafine copper powder and sodium bromide from cuprous bromide hazardous waste, while realizing the recovery of reducing metals such as the added reducing agent zinc powder, and prepares high-purity zinc oxide powder. The purity of zinc oxide is greater than 99.9% through processes such as sodium carbonate precipitation and high-temperature calcination. Compared with the same type of process, the high-temperature calcination plus one-time ammonia evaporation process is adopted, the operation process is short, the process is relatively simple, and the product purity is high.

[0032] In summary, the present invention not only improves the utilization rate of raw materials, but also realizes the efficient recovery of various substances, has good application prospects and promotion value, is suitable for treating organic solvent systems containing catalytic metal halogen compounds, and realizes the recovery of halogen elements and catalytic metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a flow chart of the preparation process. DETAILED DESCRIPTION

[0034] In order to make the above and other purposes, features, and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with specific embodiments. The test materials, reagents, etc. used in the following examples can be obtained through commercial channels or known experimental methods.

[0035] The following are specific embodiments of the present invention, but are not limited thereto:

[0036] 1. Implementation methods of hazardous waste pretreatment:

[0037] 1.1. Choice of cleaning agent

[0038] The solvents that are more effective for dissolving DMAC are generally dichloromethane, ethyl acetate, methanol and acetone. Take 100g of solid waste (residue produced by falling film evaporation of the filtrate after zincification and precipitation filtration in the tetrafluorobutadiene production process), wash it with 1:1 pure solvent for 30 minutes, detect the bromine content in the liquid after washing and the DMAC content in the solid after washing, calculate the cuprous bromide loss rate and DMAC removal rate, and the washing effect is as follows:

[0039] Cleaning agent Dichloromethane Ethyl acetate Methanol acetone Cuprous bromide loss rate 41.34% 5.88% 37.52% 73.26% DMAC removal rate 77.59% 41.23% 94.31% 56.43% Difficulty of the process Volatile and difficult to clean Easy to clean Easier to clean Easy to clean

[0040] Dichloromethane and acetone have high cuprous bromide loss rates. Dichloromethane and acetone can be excluded according to actual conditions. Ethyl acetate and methanol need to be combined in proportion to achieve the maximum cleaning effect. According to the above experimental results, it is believed that ethyl acetate should be used as the base liquid. The effect of the amount of methanol added on the cleaning effect is as follows:

[0041] Methanol addition amount 2% 4% 6% 8% 10% 12% 14% 16% Cuprous bromide loss rate% 4.56 5.28 6.01 6.38 7.53 9.86 13.26 18.96 DMAC removal rate% 65.69 73.87 80.13 85.12 84.66 83.27 84.79 85.31

[0042] Through the above implementation, when the amount of methanol added reaches 8%, the removal rate of DMAC stabilizes at about 85%, but continued addition will lead to the loss of cuprous bromide, so the optimal addition amount is 8%.

[0043] 1.2.Choice of cleaning ratio

[0044] Different cleaning ratios have a great influence on the cleaning effect. Therefore, we designed cleaning ratios of 1:1, 1:1.5, 1:2, 1:2.5, and 1:3. The cleaning results after 30 minutes of cleaning with 8% methanol addition are as follows:

[0045] Cleaning ratio 1:1 1:1.5 1:2 1:2.5 1:3 Cuprous bromide loss rate% 6.42 7.38 11.67 18.92 24.44 DMAC removal rate% 85.49 90.31 92.27 93.14 94.26

[0046] As the cleaning ratio increases, the cuprous bromide loss rate increases rapidly, and the DMAC removal rate does not change significantly. Therefore, the greatest economic benefit is achieved under a 1:1.5 cleaning ratio.

[0047] 1.3.Choice of cleaning time

[0048] The cleaning time will affect the removal rate of DMAC, so we implemented cleaning for 30min, 60min, 90min, 120min, and 150min. The results of the addition of 8% methanol and a dosing ratio of 1:1.5 are as follows:

[0049] Cleaning time 30min 60min 90min 120min 150min Cuprous bromide loss rate% 7.53 7.66 7.78 7.75 8.02 DMAC removal rate% 90.26 92.55 94.18 96.47 95.83

[0050] Through the above implementation, the maximum DMAC removal rate and the lower cuprous bromide loss rate were achieved when the cleaning time was 120 min.

[0051] In summary, using ethyl acetate with 8% methanol added as the cleaning agent and cleaning for 120 minutes at a cleaning ratio of 1:1.5 has the best effect on the pretreatment of hazardous waste.

[0052] 2. Reduction reaction

[0053] Zinc powder is used as the reducing agent; the pretreated cuprous bromide hazardous waste solid is added into the reaction tank, dispersed in water at a ratio of 1:1, stirred and then added with the reducing agent for reaction, with a stirring speed of 200-1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80-90°C, and the reaction time is 1-8h; during the reaction, isomeric tridecanol, propylene glycol, n-butanol or phenylethanol dispersant is sprayed.

[0054] 3. Separation and purification implementation methods

[0055] After the reduction reaction is completed, the reaction product is separated from the unreacted substance by filtering or centrifuging, and the obtained solid is a crude ultrafine copper powder, and the liquid is a solution containing sodium bromide.

[0056] 4. Sodium bromide solution pretreatment and electrolysis

[0057] The sodium bromide solution is pretreated by dichloromethane extraction or sodium hypochlorite oxidation to remove most of the residual organic matter; and bromine is prepared by electrolysis.

[0058] 5. Methods of zinc oxide recovery

[0059] After electrolysis, most of the COD in the wastewater is degraded, but there are still a lot of organic matter. Therefore, when using sodium carbonate solution to precipitate zinc ions in the solution, zinc carbonate will adsorb organic matter in the solution, resulting in low purity of the precipitated zinc carbonate product. Therefore, zinc carbonate is first calcined to burn off most of the organic matter, and then ammonia water is used to dissolve zinc oxide, and impurities are filtered to obtain a high-purity zinc oxide solution. Ammonia is evaporated at 95°C to precipitate zinc oxide to achieve high-purity zinc oxide.

[0060] The relationship between calcination temperature and zinc oxide purity is as follows:

[0061] Calcination temperature / ℃ 200 250 300 350 400 450 Zinc oxide purity / % 48.95 63.12 90.77 94.46 96.88 98.79

[0062] Zinc carbonate decomposes in large quantities at 300°C and is basically completely decomposed at 350°C, but the organic matter is not completely calcined, affecting the purity of zinc oxide. By continuously increasing the calcination temperature, the purity can be improved and the content of organic matter can be reduced. The calcined zinc oxide is then purified with ammonia water, which can effectively separate and remove organic matter and improve product purity.

[0063] The following is the relationship between the amount of ammonia added and the recovery rate of zinc oxide:

[0064] Ammonia addition amount 1:1 2.5:1 5:1 7.5:1 10:1 12.5:1 Zinc oxide recovery rate / % 37.98 64.56 85.69 91.17 96.66 98.23

[0065] The greater the amount of ammonia added, the more zinc oxide dissolves. According to actual conditions, the maximum economic recovery rate of zinc oxide can be achieved by adding ammonia in a ratio of 10:1.

[0066] The ammonia water that dissolves zinc oxide is the zinc oxide mother liquor. The zinc oxide is precipitated by evaporating the mother liquor to recover ammonia, thereby achieving the purification of zinc oxide. The following is the relationship between the ammonia evaporation temperature and the zinc oxide yield:

[0067] Ammonia evaporation temperature / ℃ 75 80 85 90 95 100 Zinc oxide yield / % 90.26 92.11 95.38 97.86 98.21 99.02

[0068] When the ammonia evaporation temperature reaches 95°C, the zinc oxide recovery rate is greater than 98%. Therefore, the use of high-temperature ammonia evaporation at 95°C can achieve rapid separation of ammonia and a higher zinc oxide recovery rate. The purity of zinc oxide after purification is greater than 99.9%.

[0069] 6. Product quality

[0070] Zinc Oxide:

[0071] Serial number project index 1 Zinc oxide content, w / % ≥99.90 2 Moisture, w / % ≤0.1 3 Loss on ignition, w / % ≤0.01

[0072] The applicant declares that, based on the above embodiments, technicians in the relevant technical field combine the specific content point value of a component in the above embodiments with the technical solutions in the content of the invention to produce a new numerical range, which is also one of the recorded ranges of the present invention. In order to make the specification concise, the present application no longer lists these numerical ranges.

Claims

1. A process for preparing zinc oxide using DMAC cuprous bromide hazardous waste, characterized in that: The steps include: Step 1: Raw material preparation Collect cuprous bromide hazardous waste and conduct preliminary sorting to remove impurities and pollutants; Step 2: Grinding and pretreatment The cuprous bromide hazardous waste is ground and passed through a 60-mesh sieve, and then cleaned with a special organic solvent cleaning solution containing 2-16% methanol; the ratio of hazardous waste to cleaning solution is 1:1-1:3, and the cleaning time is 30-150 minutes; after cleaning, the solid is stored for use in subsequent processes; Step 3: Reduction reaction The pretreated cuprous bromide hazardous waste solid is added to the reaction tank, dispersed in water at a ratio of 1:1, stirred and then added with a reducing agent for reaction, the stirring speed is 200-1600rps; the reducing agent is zinc powder, the reaction temperature is 80-90°C, and the reaction time is 1-8h; during the reaction, an alcohol dispersant such as isomeric tridecanol or phenylethanol is sprayed; Step 4: Separation and purification After the reduction reaction is completed, the reaction product is separated from the unreacted substance by filtering or centrifugation, and the obtained solid is a crude ultrafine copper powder, and the liquid is a solution containing sodium bromide; Step 5: Sodium bromide solution pretreatment and electrolysis Pre-treating the sodium bromide solution by dichloromethane extraction or sodium hypochlorite oxidation to remove most of the residual organic matter; and electrolyzing to prepare bromine; Step 6: Recovery of zinc oxide Adding sodium carbonate solution to the waste liquid after electrolysis in step 5 to precipitate zinc ions, filtering and separating solids; preparing zinc oxide by high-temperature calcination; purifying the calcined zinc oxide by ammonia water, and purifying the zinc oxide by ammonia evaporation process; Step 7: Product Testing The recycled zinc oxide is quality tested to ensure that the product meets relevant standards.

2. A process for preparing zinc oxide using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the grinding and pretreatment of step 2, a special organic solvent cleaning solution containing 8% methanol is used to clean the cuprous bromide hazardous waste, the ratio of hazardous waste to cleaning solution is 1:1~1:1.5, and the cleaning time is 120 minutes.

3. A process for preparing zinc oxide using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the reduction reaction of step 3, zinc powder is used as the reducing agent; the stirring speed is 1400-1600 rps; the reaction time is 4 h; and 1-3% of isotridecyl alcohol is sprayed during the reaction.

4. A process for preparing zinc oxide using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the recovery of zinc oxide in step 6, the calcination temperature is 300-450°C; the ratio of the amount of ammonia water added to zinc oxide is 10:1; and the temperature of the ammonia evaporation process is 95-105°C.

5. The application of the sodium bromide process as claimed in claim 1, characterized in that: The preparation process is applied to an organic solvent system of a halogen compound containing a catalytic metal; the catalytic metal includes nickel, copper, silver, gold, platinum or palladium.