Recycled concrete pile used in freeze-thaw environment and preparation method thereof
By using silica fume to replace cement, recycled coarse aggregate to replace natural coarse aggregate, and adding polypropylene fine fibers and calcium chloride in recycled concrete, the problem of insufficient frost resistance of recycled concrete in high-cold areas in the existing technology is solved. Significantly improved frost resistance and structural stability.
Patent Information
- Application Number
- CN202410807807.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
Existing recycled concrete has insufficient frost resistance in freeze-thaw environments in alpine regions and cannot meet the needs of pile foundation structures that have been exposed to long-term freezing.
Use silica fume to partially replace cement, use recycled coarse aggregate to replace natural coarse aggregate, and add polypropylene fine fibers and calcium chloride. The amount of calcium chloride added is 0.5-1.5% of the total mass of cement and silica fume. Polypropylene The addition amount of fine fibers is 0.5-1.5%, which improves the frost resistance by improving the bonding force and structural compactness of concrete.
It significantly improves the frost resistance of recycled concrete, reduces the formation of pores and cracks caused by freeze-thaw cycles, extends the service life of the structure, and meets the stability needs of soft foundation soil in alpine areas.
Smart Images

Figure CN118724531A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycled concrete, and in particular relates to a recycled concrete pile used in a freeze-thaw environment and a preparation method thereof. Background Art
[0002] At present, green resource recycling has become an important means of sustainable development and green environmental protection. Using recycled aggregates produced from waste concrete to prepare recycled concrete can not only solve the current problem of resource shortage, but also achieve the goals of recycling resources and protecting the environment. It is a necessary measure for the further healthy development of the construction industry.
[0003] For high-altitude cold areas, foundation buildings and the like will suffer different degrees of freeze-thaw damage due to the large temperature difference. Therefore, when using recycled concrete materials to prepare concrete piles, it is necessary to ensure that the recycled concrete itself has a strong ability to resist freeze-thaw damage and does not suffer freeze-thaw damage within the service life. Recycled concrete piles used in freeze-thaw environments are piles made of concrete (including ordinary natural concrete and recycled concrete) to strengthen the foundation stability of soil layers in soft silt areas in cold regions. A Chinese patent with patent application number 202210269109.X discloses a recycled concrete and preparation method that can be recycled in severe cold regions. It belongs to the field of concrete materials. The patent proposes the addition of cementitious materials such as fly ash, mineral powder and air entraining agent to improve the freeze-thaw resistance of the recycled concrete material itself, thereby improving the freeze resistance and durability of recycled concrete in cold regions to a certain extent. However, although the incorporation of these materials has improved the freeze resistance of recycled concrete to a certain extent, for pile foundation structures that have been frozen for a long time, the above materials still cannot meet the demand. Summary of the invention
[0004] In order to meet the demand for stability of soft foundation soil layers in high-cold areas, the present invention proposes a regenerated concrete pile for use in a freeze-thaw environment and a preparation method thereof. The present invention has the advantages of freeze-thaw resistance, simple preparation, green environmental protection, and resource conservation.
[0005] To achieve the above-mentioned purpose, the present invention provides a regenerated concrete pile for use in a freeze-thaw environment, wherein cement is partially replaced by silica fume, natural coarse aggregate is partially replaced by recycled coarse aggregate, and polypropylene fine fibers and calcium chloride are added; wherein the amount of calcium chloride added is 0.5-1.5% of the total mass of the cement and silica fume; the amount of polypropylene fine fibers added is 0.5-1.5% (that is, the amount of polypropylene fine fibers added is 0.5-1.5% of the total volume of the natural coarse aggregate, recycled coarse aggregate, river sand, cement, silica fume, water reducer, water and polypropylene fine fibers).
[0006] Furthermore, the particle size of the natural coarse aggregate is 4.75-20 mm, and the particle size of the recycled coarse aggregate is 4.75-20 mm; the replacement rate of the recycled coarse aggregate for the natural coarse aggregate is 50%.
[0007] Furthermore, the mass ratio of cement to silica fume is (26-27): (362-369).
[0008] Furthermore, the following raw materials are included by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate, 667 parts of river sand, 362-369 parts of cement, 26-27 parts of silica fume, 4-5 parts of water reducer and 175 parts of water, and also include polypropylene fine fibers and calcium chloride.
[0009] Furthermore, the recycled coarse aggregate is Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate specified in GB / T25177-2010.
[0010] Furthermore, the particle size of the river sand is less than 4.75 mm and the fineness modulus is 2.62.
[0011] Furthermore, the cement is ordinary Portland cement.
[0012] Furthermore, the SiO 2 Content ≥90%.
[0013] Furthermore, the water reducing agent is a polycarboxylic acid-based water reducing agent.
[0014] Furthermore, the polypropylene fine fiber has a length of 12 mm and a diameter of 48 μm.
[0015] The present invention also proposes a method for preparing the regenerated concrete piles in a freeze-thaw environment, comprising the following steps:
[0016] Weigh each raw material by weight, put natural coarse aggregate, recycled coarse aggregate and river sand into a mixer and stir evenly, add 50wt% of water and continue stirring, then add cement, silica fume, polypropylene fine fiber, calcium chloride and the remaining water into the mixer and stir evenly, finally add a water reducer and stir to obtain a recycled concrete mixture, mold the recycled concrete mixture, perform standard maintenance after demolding, and obtain the recycled concrete pile for use in a freeze-thaw environment.
[0017] Furthermore, the standard curing is to place the product in water for curing for 4 days at 20±2°C and relative humidity of 95% or more for 24 days.
[0018] Compared with the prior art, the present invention has the following advantages and technical effects:
[0019] (1) The present invention can activate volcanic ash by increasing the amount of silica fume to replace a certain amount of cement, thereby converting the unfavorable calcium hydroxide in concrete into favorable CSH gel, improving the bonding between the paste and the aggregate interface; and the use of water reducer can improve the fluidity of the concrete mixture and improve the homogeneity of the concrete; in addition, the present invention also adds polypropylene fine fiber material, and the addition of polypropylene fine fiber in the recycled concrete can effectively inhibit the formation and development of cracks in the hardening stage of concrete. The main effect is that the polypropylene fine fiber can form a good network structure between the aggregates, and the structure cooperates with the aggregates and cement matrix to achieve the effect of limiting the lateral deformation of the internal pore structure. The polypropylene fine fiber has good ductility and can improve the bonding force between the coarse and fine aggregates and the mortar, thereby reducing the pores and cracks generated in the recycled concrete due to the freeze-thaw cycle; and calcium chloride can absorb water vapor in the air, so that the concrete can continuously maintain a certain moderate humidity, which can further play the secondary hydration of cement and the added volcanic ash material, improve the strength, stability and density of the recycled concrete, and thus improve the anti-freeze performance. .
[0020] (2) In the preparation process of the present invention, the raw materials are mixed in batches and stirred sufficiently to allow the raw materials to fully cooperate and play a role. The method is simple, efficient, and has the characteristics of simple production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0022] Figure 1 The elastic modulus changes of each group of recycled concrete specimens after different freeze-thaw cycles;
[0023] Figure 2 The changes in the apparent characteristics of the specimens of Example 1 (RC-J1C1), Example 3 (RC-J1.5C1.5) and Comparative Example 1 (RC-J0C0) after 50, 100 and 150 freeze-thaw cycles;
[0024] Figure 3 The mass loss rate curve of each group of recycled concrete specimens after different freeze-thaw cycles;
[0025] Figure 4 This is the relative dynamic elastic modulus loss rate curve of each group of recycled concrete specimens after different freeze-thaw cycles. DETAILED DESCRIPTION
[0026] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0027] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0028] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0029] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0030] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0031] The embodiment of the present invention provides a regenerated concrete pile for use in a freeze-thaw environment, wherein cement is partially replaced by silica fume, natural coarse aggregate is partially replaced by recycled coarse aggregate, and polypropylene fine fibers and calcium chloride are added; wherein the amount of calcium chloride added is 0.5-1.5% of the total mass of the cement and silica fume; and the amount of polypropylene fine fibers added is 0.5-1.5%.
[0032] The invention comprises the following raw materials by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate, 667 parts of river sand, 362-369 parts of cement, 26-27 parts of silica fume, 4-5 parts of water reducer and 175 parts of water, and also comprises polypropylene fine fiber and calcium chloride. The amount of the polypropylene fine fiber added is 0.5-1.5% of the total volume of the natural coarse aggregate, recycled coarse aggregate, river sand, cement, silica fume, water reducer, water and polypropylene fine fiber, and the amount of the calcium chloride added is 0.5-1.5% of the total mass of the cement and silica fume.
[0033] In a preferred embodiment of the present invention, the particle size of the natural coarse aggregate is 4.75-20 mm, and the particle size of the recycled coarse aggregate is 4.75-20 mm; the replacement rate of the recycled coarse aggregate for the natural coarse aggregate is 50%.
[0034] In a preferred embodiment of the present invention, the mass ratio of cement to silica fume is (26-27): (362-369).
[0035] In a preferred embodiment of the present invention, the recycled coarse aggregate is Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate specified in GB / T25177-2010.
[0036] In a preferred embodiment of the present invention, the raw materials include, by weight, 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate, 667 parts of river sand, 362-369 parts of cement, 26-27 parts of silica fume, 4-5 parts of water reducer and 175 parts of water.
[0037] In a preferred embodiment of the present invention, the river sand is medium sand with a particle size less than 4.75 mm and a fineness modulus of 2.62.
[0038] In a preferred embodiment of the present invention, the cement is ordinary Portland cement (P.042.5, purchased from Huaxin Cement (Ezhou) Co., Ltd.), with a density of 3150 kg / m 3 , the 28d compressive strength is 47.9MPa.
[0039] In a preferred embodiment of the present invention, the silica fume is an ultrafine amorphous byproduct of silicon processing, purchased from Hubei Wuhan Zhongjian Commercial Concrete Co., Ltd., and its apparent density is 2700kg / m 3 , with a specific surface area of 23000m 2 / kg,SiO 2 Content ≥90%.
[0040] In a preferred embodiment of the present invention, the water reducer is a polycarboxylic acid-based water reducer with a water reduction efficiency of 20-30%, and the purchase manufacturer is Shanxi Feike New Material Technology Co., Ltd.
[0041] In a preferred embodiment of the present invention, the polypropylene fine fiber has a length of 12 mm, a diameter of 48 μm, a tensile strength of 358 MPa, and is purchased from Shanghai Chenqi Chemical Technology Co., Ltd.
[0042] In a preferred embodiment of the present invention, the calcium chloride is white powder particles with a net content of 96%, and the manufacturer is Sinopharm Chemical Reagent Co., Ltd.
[0043] The embodiment of the present invention further proposes a method for preparing the regenerated concrete pile in a freeze-thaw environment, comprising the following steps:
[0044] Weigh each raw material by weight, put natural coarse aggregate, recycled coarse aggregate and river sand into a mixer and stir evenly, add 50wt% of water and continue stirring, then add cement, silica fume, polypropylene fine fiber, calcium chloride and the remaining water into the mixer and stir evenly, finally add a water reducer and stir to obtain a recycled concrete mixture, mold the recycled concrete mixture, perform standard maintenance after demolding, and obtain the recycled concrete pile for use in a freeze-thaw environment.
[0045] In a preferred embodiment of the present invention, the standard curing is to place the product in water for curing in a water bath for 4 days after being kept at 20±2°C and a relative humidity of 95% or higher for 24 days.
[0046] In a preferred embodiment of the present invention, the size of the mold used for molding is 100 mm×100 mm×300 mm.
[0047] In the embodiment of the present invention, the volume replacement amount of polypropylene fine fibers refers to the percentage of the added amount of polypropylene fine fibers to the total volume of natural coarse aggregate, recycled coarse aggregate, river sand, cement, silica fume, water reducer, water and polypropylene fine fibers, and the added amount of calcium chloride refers to the percentage of the added amount of calcium chloride to the total mass of cement and silica fume.
[0048] The technical solution of the present invention is further illustrated by the following embodiments.
[0049] Example 1
[0050] Weigh the following raw materials by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate), 667 parts of river sand, 366.37 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and also weigh polypropylene fine fiber (volume replacement amount is 0.5%) and calcium chloride (addition amount is 0.5%, that is, the amount of calcium chloride added is 0.5% of the total mass of cement and silica fume);
[0051] In order, put natural coarse aggregate, recycled coarse aggregate and river sand into the mixer and mix for 60 seconds until uniform;
[0052] Add 50 wt% water into the mixer and continue stirring for 60 seconds;
[0053] Continue to add cement, silica fume, polypropylene fine fiber, calcium chloride and the remaining water into the mixer and stir for 60 seconds until uniform;
[0054] Finally, the water reducing agent was added into the mixer and stirred for 60 seconds until uniform to obtain a recycled concrete mixture;
[0055] The obtained recycled concrete mixture is placed in a plastic mold with a size of 100 mm × 100 mm × 300 mm for molding, and then vibrated, centrifuged and compacted. The inner wall of the mold is coated with lubricating oil in advance to facilitate subsequent demoulding;
[0056] The recycled concrete after curing was demolded and then placed in a curing box for standard curing (temperature 20±2°C, relative humidity above 95%) for 24 days, and then placed in water for water bath curing for 4 days to obtain recycled concrete piles for use in freeze-thaw environments, recorded as RC-J0.5C0.5.
[0057] Example 2
[0058] Weigh the following raw materials by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 364.4 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and also weigh polypropylene fine fiber (volume substitution amount is 1.0%) and calcium chloride (addition amount is 1.0%);
[0059] In order, put natural coarse aggregate, recycled coarse aggregate and river sand into the mixer and mix for 60 seconds until uniform;
[0060] Add 50 wt% water into the mixer and continue stirring for 60 seconds;
[0061] Continue to add cement, silica fume, polypropylene fine fiber, calcium chloride and the remaining water into the mixer and stir for 60 seconds until uniform;
[0062] Finally, the water reducing agent was added into the mixer and stirred for 60 seconds until uniform to obtain a recycled concrete mixture;
[0063] The obtained recycled concrete mixture is placed in a plastic mold with a size of 100 mm × 100 mm × 300 mm for molding, and then vibrated, centrifuged and compacted. The inner wall of the mold is coated with lubricating oil in advance to facilitate subsequent demoulding;
[0064] The recycled concrete after curing was demolded and then placed in a curing box for standard curing (temperature 20±2°C, relative humidity above 95%) for 24 days, and then placed in water for water bath curing for 4 days to obtain recycled concrete piles for use in freeze-thaw environments, recorded as RC-J1C1.
[0065] Example 3
[0066] Weigh the following raw materials by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and also weigh polypropylene fine fiber (volume replacement amount is 1.5%) and calcium chloride (addition amount is 1.5%);
[0067] In order, put natural coarse aggregate, recycled coarse aggregate and river sand into the mixer and mix for 60 seconds until uniform;
[0068] Add 50 wt% water into the mixer and continue stirring for 60 seconds;
[0069] Continue to add cement, silica fume, polypropylene fine fiber, calcium chloride and the remaining water into the mixer and stir for 60 seconds until uniform;
[0070] Finally, the water reducing agent was added into the mixer and stirred for 60 seconds until uniform to obtain a recycled concrete mixture;
[0071] The obtained recycled concrete mixture is placed in a plastic mold with a size of 100 mm × 100 mm × 300 mm for molding, and then vibrated, centrifuged and compacted. The inner wall of the mold is coated with lubricating oil in advance to facilitate subsequent demoulding;
[0072] The recycled concrete after curing was demolded and then placed in a curing box for standard curing (temperature 20±2°C, relative humidity above 95%) for 24 days, and then placed in water for water bath curing for 4 days to obtain recycled concrete piles for use in freeze-thaw environments, recorded as RC-J1.5C1.5.
[0073] Example 4
[0074] The same as Example 1, except that the following raw materials are weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fibers (volume substitution amount is 0.5%) and calcium chloride (addition amount is 1%) are weighed;
[0075] The obtained recycled concrete pile for use in freeze-thaw environment is recorded as RC-J0.5C1.
[0076] Example 5
[0077] The same as Example 1, except that the following raw materials are weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fibers (volume substitution amount is 0.5%) and calcium chloride (addition amount is 1.5%) are weighed;
[0078] The obtained recycled concrete pile for use in freeze-thaw environment is recorded as RC-J0.5C1.5.
[0079] Example 6
[0080] The same as Example 1, except that the following raw materials are weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fibers (volume substitution amount is 1%) and calcium chloride (addition amount is 0.5%) are weighed;
[0081] The obtained recycled concrete pile for use in freeze-thaw environment is recorded as RC-J1C0.5.
[0082] Example 7
[0083] The same as Example 1, except that the following raw materials are weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fibers (volume substitution amount is 1%) and calcium chloride (addition amount is 1.5%) are weighed;
[0084] The obtained recycled concrete pile for use in freeze-thaw environment is recorded as RC-J1C1.5.
[0085] Example 8
[0086] The same as Example 1, except that the following raw materials are weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fibers (volume substitution amount is 1.5%) and calcium chloride (addition amount is 0.5%) are weighed;
[0087] The obtained recycled concrete pile for use in freeze-thaw environment is recorded as RC-J1.5C0.5.
[0088] Example 9
[0089] The same as Example 1, except that the following raw materials are weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fibers (volume substitution amount is 1.5%) and calcium chloride (addition amount is 1%) are weighed;
[0090] The obtained recycled concrete pile for use in freeze-thaw environment is recorded as RC-J1.5C1.
[0091] Comparative Example 1
[0092] Weigh the following raw materials by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate, 667 parts of river sand, 362.42 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer and 175 parts of water;
[0093] In order, put natural coarse aggregate, recycled coarse aggregate and river sand into the mixer and mix for 60 seconds until uniform;
[0094] Add 50 wt% water into the mixer and continue stirring for 60 seconds;
[0095] Continue to add cement, silica fume and remaining water into the mixer and stir for 60 seconds until uniform;
[0096] Finally, the water reducing agent was added into the mixer and stirred for 60 seconds until uniform to obtain a recycled concrete mixture;
[0097] The obtained recycled concrete mixture is placed in a plastic mold with a size of 100 mm × 100 mm × 300 mm for molding, and then vibrated, centrifuged and compacted. The inner wall of the mold is coated with lubricating oil in advance to facilitate subsequent demoulding;
[0098] The recycled concrete after curing was demolded and then placed in a curing box for standard curing (temperature 20±2°C, relative humidity above 95%) for 24 days, and then placed in water for water bath curing for 4 days to obtain recycled concrete piles for use in freeze-thaw environments, recorded as RC-J0C0.
[0099] Comparative Example 2
[0100] Weigh the following raw materials by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 364.4 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and weigh calcium chloride (addition amount is 1.0%);
[0101] In order, put natural coarse aggregate, recycled coarse aggregate and river sand into the mixer and mix for 60 seconds until uniform;
[0102] Add 50 wt% water into the mixer and continue stirring for 60 seconds;
[0103] Continue to add cement, silica fume, calcium chloride and the remaining water into the mixer and stir for 60 seconds until uniform;
[0104] Finally, the water reducing agent was added into the mixer and stirred for 60 seconds until uniform to obtain a recycled concrete mixture;
[0105] The obtained recycled concrete mixture is placed in a plastic mold with a size of 100 mm × 100 mm × 300 mm for molding, and then vibrated, centrifuged and compacted. The inner wall of the mold is coated with lubricating oil in advance to facilitate subsequent demoulding;
[0106] The recycled concrete after curing was demolded and then placed in a curing box for standard curing (temperature 20±2°C, relative humidity above 95%) for 24 days, and then placed in water for water bath curing for 4 days to obtain recycled concrete piles for use in freeze-thaw environments, recorded as RC-J0C1.
[0107] Comparative Example 3
[0108] The following raw materials were weighed in parts by weight: 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate (Class I recycled coarse aggregate, Class II recycled coarse aggregate or Class III recycled coarse aggregate), 667 parts of river sand, 364.4 parts of cement, 26.65 parts of silica fume, 4.2 parts of water reducer, 175 parts of water, and polypropylene fine fiber (volume substitution amount is 1.0%);
[0109] In order, put natural coarse aggregate, recycled coarse aggregate and river sand into the mixer and mix for 60 seconds until uniform;
[0110] Add 50 wt% water into the mixer and continue stirring for 60 seconds;
[0111] Continue to add cement, silica fume, polypropylene fine fiber and remaining water into the mixer and stir for 60 seconds until uniform;
[0112] Finally, the water reducing agent was added into the mixer and stirred for 60 seconds until uniform to obtain a recycled concrete mixture;
[0113] The obtained recycled concrete mixture is placed in a plastic mold with a size of 100 mm × 100 mm × 300 mm for molding, and then vibrated, centrifuged and compacted. The inner wall of the mold is coated with lubricating oil in advance to facilitate subsequent demoulding;
[0114] The recycled concrete after curing was demolded and then placed in a curing box for standard curing (temperature 20±2°C, relative humidity above 95%) for 24 days, and then placed in water for water bath curing for 4 days to obtain recycled concrete piles for use in freeze-thaw environments, recorded as RC-J1C0.
[0115] Performance Testing
[0116] According to the specification "Test Method for Long-term Performance and Durability of Ordinary Concrete" (GB / T500082-2009) and "Standard for Test Method for Mechanical Properties of Ordinary Concrete" (GBT50081-2002), the rapid freeze-thaw method was used to subject the recycled concrete pile specimens prepared in Examples 1-9 and Comparative Example 1 to 50, 100 and 150 freeze-thaw cycles. The axial compressive strength, mass and relative dynamic elastic modulus of the prismatic specimens were tested after every 50 freeze-thaw cycles, and the uniaxial static elastic modulus was calculated.
[0117] The test results of the axial compressive strength of the recycled concrete pile specimens prepared in Examples 1-9 and Comparative Example 1 before freeze-thaw cycles are shown in Table 1.
[0118] Table 1 Axial compressive strength test results of the embodiment and comparative example specimens before freeze-thaw cycles (MPa)
[0119]
[0120] The axial compressive strength test results of the recycled concrete pile specimens prepared in Examples 1-9 and Comparative Example 1 after 50 freeze-thaw cycles are shown in Table 2.
[0121] Table 2 Axial compressive strength test results after 50 freeze-thaw cycles of the embodiments and comparative examples (MPa)
[0122]
[0123] The axial compressive strength test results of the recycled concrete pile specimens prepared in Examples 1-9 and Comparative Example 1 after 100 freeze-thaw cycles are shown in Table 3.
[0124] Table 3 Axial compressive strength test results after 100 freeze-thaw cycles of the embodiments and comparative examples (MPa)
[0125]
[0126]
[0127] The axial compressive strength test results of the recycled concrete pile specimens prepared in Examples 1-9 and Comparative Example 1 after 150 freeze-thaw cycles are shown in Table 4.
[0128] Table 4 Axial compressive strength test results after 150 freeze-thaw cycles of the embodiments and comparative examples (MPa)
[0129]
[0130] It can be seen from Tables 1 to 4 that the amount of polypropylene fine fibers and inorganic calcium chloride added will affect the axial compressive strength of the recycled concrete, and the axial compressive strength of the recycled concrete mixed with polypropylene fine fibers and inorganic calcium chloride is always greater than that of the benchmark recycled concrete in Comparative Example 1.
[0131] The relationship and results of the elastic modulus changes of each group of recycled concrete specimens after different freeze-thaw cycles are shown in Figure 1 and Table 5.
[0132] Table 5 Elastic modulus test results of recycled concrete specimens after different freeze-thaw cycles (GPa)
[0133]
[0134]
[0135] From Table 5 and Figure 1 It can be seen that the uniaxial static elastic modulus of recycled concrete with different mix ratios has decreased to varying degrees after experiencing freeze-thaw cycles. With the extension of the number of freeze-thaw cycles, the double addition of polypropylene fine fibers and inorganic calcium chloride can reduce the change of the elastic modulus of recycled concrete. At the same time, the recycled concrete specimen RC-J1C1 with 1% polypropylene fine fibers and 1% inorganic calcium chloride can effectively maintain a high elastic modulus, significantly inhibiting the damage of freeze-thaw cycles to recycled concrete, and can be concluded to be the best mix ratio.
[0136] The changes in the apparent characteristics of the samples of Example 1 (RC-J1C1), Example 3 (RC-J1.5C1.5) and Comparative Example 1 (RC-J0C0) after 50, 100 and 150 freeze-thaw cycles are shown in Figure 2 Taking RC-J0C0-100 as an example, RC-J0C0-100 represents the apparent characteristics of the specimen after RC-J0C0 has undergone 100 freeze-thaw cycles. Figure 2It can be seen that after 50 freeze-thaw cycles, a small amount of cement mortar fell off the surface of the main part of the recycled concrete prism specimen, and the fine aggregate on the surface was partially exposed due to the shedding of a small amount of cement mortar; after 100 freeze-thaw cycles, the cement mortar in the main part of the recycled concrete prism specimen continued to lose further, and the main part of the specimen became very rough due to the shedding of more and more cement mortar, and bundles of polypropylene fine fibers were found to be exposed, and some tiny holes began to appear, and the edges and corners of the prism were Slight damage, the fine aggregate of the specimen is exposed more and more obviously, and less coarse aggregate can be observed; after 150 freeze-thaw cycles, the degree of shedding and erosion of the main part of the recycled concrete prism specimen has deepened sharply, the cement mortar on the surface of the specimen has basically completely fallen off, and many obvious tiny holes appear on all four sides of the specimen. The bonding force between the cement mortar and the aggregate inside the specimen is further reduced, resulting in slight cracks on the surface of the specimen. The coarse aggregate can be clearly observed in the recycled concrete specimen, and the edges and corners of the specimen are obviously damaged. The exposed aggregate, corner damage and pore cracks of the control group specimen RC-J0C0 recycled concrete are the most obvious, while the appearance characteristics of the recycled concrete mixed with 1% polypropylene fine fiber and 1% inorganic calcium chloride change the most slowly, with fewer holes and cracks on the surface, and the damage to the corners is lighter, and the specimen still has good appearance integrity. It can be concluded that recycled concrete mixed with appropriate amounts of polypropylene fine fiber and inorganic calcium chloride can show good antifreeze performance.
[0137] The mass loss rate change curves of each group of recycled concrete specimens after different freeze-thaw cycles are shown in Figure 3 , the relative dynamic elastic modulus loss rate curve is shown in Figure 4, combined with the analysis of the freeze-thaw damage mechanism of recycled concrete, the hydrostatic pressure on recycled concrete during the freeze-thaw cycle will flow and extend along the pores and cracks inside the structure. When the flow distance of the internal pore water reaches the maximum, the hydrostatic pressure cannot continue to flow inside the structure and begins to act on the pore wall. When the hydrostatic pressure gradually increases and exceeds the tensile strength of the pore wall, the pore wall will be damaged and cause freeze-thaw damage. By adding polypropylene fine fibers, a three-dimensional random support mesh structure can be formed inside the recycled concrete structure, which can not only bear the external force on the recycled concrete, but also improve the bonding between coarse and fine aggregates and cement mortar, which can significantly improve the anti-freeze performance of recycled concrete and slow down the freeze-thaw damage process. At the same time, the use of inorganic calcium chloride can make the early hydration reaction of cement more complete, and the volcanic ash material-silica fume is also added in this experiment. Inorganic calcium chloride can make the volcanic ash effect more obvious, generate more stable hydration products to fill the structural pores inside the concrete, and form more stable and tiny closed bubbles in the internal structure to reduce the hydrostatic pressure during the freeze-thaw cycle and reduce the development of internal cracks in the recycled concrete, thereby improving the frost resistance of the recycled concrete. The relative dynamic elastic modulus of the specimen RC-J1.5C1.5 also decreased significantly. This is due to the excessive addition of polypropylene fine fibers. During the mixing and pouring of recycled concrete, the polypropylene fine fibers are unevenly dispersed and agglomerated with aggregates and cement mortar, resulting in uneven internal structure and huge defects. After molding, more cracks will be generated in the internal structure. Secondly, with the increase in the amount of inorganic calcium chloride, the hydration products produce more and more expansive calcium aluminate and complex salts during the freeze-thaw cycle, and the internal pores of the recycled concrete expand more, which leads to an accelerated decrease in the relative dynamic elastic modulus.
[0138] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A regenerated concrete pile for use in a freeze-thaw environment, characterized in that: The cement is partially replaced by silica fume, the natural coarse aggregate is partially replaced by recycled coarse aggregate, and polypropylene fine fibers and calcium chloride are added; wherein the added amount of calcium chloride is 0.5-1.5% of the total mass of the cement and silica fume; and the added amount of the polypropylene fine fibers is 0.5-1.5%.
2. The regenerated concrete pile for use in freeze-thaw environment according to claim 1, characterized in that: The particle size of the natural coarse aggregate is 4.75-20 mm, and the particle size of the recycled coarse aggregate is 4.75-20 mm; the replacement rate of the recycled coarse aggregate for the natural coarse aggregate is 50%.
3. The regenerated concrete pile for use in a freeze-thaw environment according to claim 1, characterized in that: The mass ratio of the cement to silica fume is (26-27): (362-369).
4. The regenerated concrete pile for use in a freeze-thaw environment according to claim 1, characterized in that: The raw materials include, by weight, 568 parts of natural coarse aggregate, 568 parts of recycled coarse aggregate, 667 parts of river sand, 362-369 parts of cement, 26-27 parts of silica fume, 4-5 parts of water reducer and 175 parts of water; the particle size of the river sand is less than 4.75 mm, and the fineness modulus is 2.
62.
5. The regenerated concrete pile for use in freeze-thaw environment according to claim 1, characterized in that: The cement is ordinary Portland cement.
6. The regenerated concrete pile for use in freeze-thaw environment according to claim 1, characterized in that: The SiO2 content of the silica fume is ≥90%.
7. The regenerated concrete pile for use in freeze-thaw environment according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent.
8. The regenerated concrete pile for use in freeze-thaw environment according to claim 1, characterized in that: The polypropylene fine fibers have a length of 12 mm and a diameter of 48 μm.
9. A method for preparing a regenerated concrete pile for use in a freeze-thaw environment according to any one of claims 1 to 8, characterized in that: The following steps are involved: Weigh each raw material by weight, put natural coarse aggregate, recycled coarse aggregate and river sand into a mixer and stir evenly, add 50wt% of water and continue stirring, then add cement, silica fume, polypropylene fine fiber, calcium chloride and the remaining water into the mixer and stir evenly, finally add a water reducer and stir to obtain a recycled concrete mixture, mold the recycled concrete mixture, perform standard maintenance after demolding, and obtain the recycled concrete pile for use in a freeze-thaw environment.
10. The method for preparing regenerated concrete piles for use in freeze-thaw environments according to claim 9, characterized in that: The standard curing is to place the product in water for 4 days under the conditions of 20±2°C and relative humidity of 95% or more for 24 days.