Preparation method of pentaerythritol stearate emulsion

Pentaerythritol stearate emulsion is prepared by using toluenesulfonic acid and other catalysts and water pump intermittent decompression dehydration reaction in the direct esterification method, combined with cold sodium bicarbonate washing and ethanol recrystallization, which solves the problem of long reaction time and high energy consumption. problem, achieving high catalytic activity and environmentally friendly industrial production.

CN118724706AInactive Publication Date: 2024-10-01GUANGZHOU ZHENGHAO NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410714014.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing direct esterification method for synthesizing pentaerythritol stearate requires a long reaction time and high temperature, which poses high temperature risks and high energy consumption. The catalyst activity is low, which affects product quality.

Method used

Using catalysts such as toluenesulfonic acid, the pentaerythritol stearate emulsion is prepared through intermittent decompression dehydration reaction with water pump, combined with cold sodium bicarbonate washing and ethanol recrystallization, and finally emulsified in deionized water to optimize the catalytic activity and production process.

Benefits of technology

The catalytic activity is improved, the reaction time is shortened, energy consumption is reduced, the product is easy to separate, the catalyst is degradable, there is zero VOC, and it has good industrial application prospects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of pentaerythritol stearate, and particularly relates to a pentaerythritol stearate emulsion preparation method, which comprises the following raw material components: 20-40 parts of stearic acid, 10-20 parts of a catalyst, 20-40 parts of pentaerythritol, 5-10 parts of an emulsifier, 0.5-1 part of an antifoaming agent, 0.5-1 part of a preservative, and 10-50 parts of deionized water. According to the invention, pentaerythritol and stearic acid are used as raw materials, the synthesis and modification of pentaerythritol stearate under a solvent-free condition are researched, and the influence of different reaction conditions on the yield is explored. The synthesis method has the advantages that the catalytic yield is high, the product is easy to separate, the catalyst has degradability, zero VOC (volatile organic compound) and no pollution, and the like, and has a very good industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pentaerythritol stearate, and particularly relates to a preparation method of a pentaerythritol stearate emulsion. Background Art

[0002] Mineral lubricants are petroleum products whose resources are becoming increasingly depleted. During use, they enter the environment due to splashing, leakage, and expiration replacement. Their degradation rate in nature is only 10-33%, and they can pollute groundwater for more than 100 years. Cool lubricants based on natural animal and plant oils are renewable, easily biodegradable, and have excellent lubrication properties. They are potential ideal substitutes for mineral lubricants and have attracted much attention from researchers at home and abroad.

[0003] The synthesis methods of fatty acid esters include direct esterification, transesterification, acyl chloride, etc. The esterification method is not only convenient and fast, but also has a high esterification rate. Scholars at home and abroad have carried out related research work. Pentaerythritol tetrastearate was synthesized by direct esterification, and mesoporous SnO-y-Al, O3 composite materials were prepared by seed crystallization method as solid acid catalysts. The coke formation was delayed during the reaction, and the conversion rate of pentaerythritol and the selectivity of pentaerythritol tetrastearate were significantly improved. However, the direct esterification method has a long reaction time and a high reaction temperature, and has certain high temperature hazards and large energy consumption. Therefore, it is necessary to explore a process route for pentaerythritol stearate with low energy consumption and excellent product quality.

[0004] Therefore, it is necessary to invent a method for preparing pentaerythritol stearate emulsion to solve the above problems. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for preparing a pentaerythritol stearate emulsion to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical scheme: a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 20-40 parts of stearic acid, 10-20 parts of a catalyst, 20-40 parts of pentaerythritol, 5-10 parts of an emulsifier, 0.5-1 parts of a defoaming agent, 0.5-1 parts of a preservative and 10-50 parts of deionized water, characterized in that it comprises the following specific steps:

[0007] S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add a catalyst, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0008] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0009] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0010] Furthermore, the catalyst is one of toluenesulfonic acid, aluminum oxide, aminosulfonic acid, zinc sulfate and molybdic acid.

[0011] Furthermore, the catalyst can also be a solid superacid catalyst, and its preparation method is as follows:

[0012] Dissolve ferric sulfate and stannous chloride in deionized water, add ammonia water dropwise while stirring to adjust the pH value to 8-9, filter and wash to remove harmful ions after 24 hours, dry at 115°C for 12 hours, crush and sieve, soak in sulfuric acid solution for 5 minutes, filter, dry, and roast in a 500-600°C resistance furnace for 3 hours to obtain a solid superacid catalyst.

[0013] Furthermore, the molar ratio of the ferric sulfate to the stannous chloride is 3:1, and the sulfuric acid solution is 0.5 mol·L -1 .

[0014] Furthermore, the mass percentage of ethanol in step S2 is 95%.

[0015] Furthermore, the mass percentage of the solid superacid catalyst is 1%-1.5%.

[0016] Technical effects and advantages of the present invention:

[0017] 1. Compared with the existing pentaerythritol stearate production process, the present invention shows that the chemical activity of toluenesulfonic acid is the highest, and the chemical activity rate of toluenesulfonic acid can reach 2% after 60 minutes of reaction. The chemical activity rate of the other three chemical agents is lower than 40%. It can be seen that p-toluenesulfonic acid is a better catalyst. The quaternary tetraol stearic acid is catalyzed and synthesized with p-toluenesulfonic acid as the catalyst, tetraol and stearic acid as the reactants, which has a good catalytic activity optimization effect on the product synthesis;

[0018] 2. The present invention uses pentaerythritol and stearic acid as raw materials, studies the synthesis and modification of pentaerythritol stearate under solvent-free conditions, and explores the influence of different reaction conditions on the yield. The synthesis method has the following advantages, such as high catalytic yield, easy separation of products, degradability of the catalyst, zero VOC, no pollution, etc., and has a good industrial application prospect.

[0019] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structure pointed out in the description. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1:

[0022] The present invention provides a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 20 parts of stearic acid, 10 parts of a catalyst, 30 parts of pentaerythritol, 5 parts of an emulsifier, 0.5 parts of a defoaming agent, 0.5 parts of a preservative and 35 parts of deionized water, and is characterized in that the method comprises the following specific steps:

[0023] S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add toluenesulfonic acid, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0024] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in 95% by mass ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0025] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0026] Embodiment 2:

[0027] The present invention provides a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 40 parts of stearic acid, 10 parts of a catalyst, 20 parts of pentaerythritol, 10 parts of an emulsifier, 0.5 parts of a defoaming agent, 1 part of a preservative and 18.5 parts of deionized water, and is characterized in that the method comprises the following specific steps:

[0028] S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add aluminum oxide, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0029] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in 95% by mass ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0030] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0031] Embodiment 3:

[0032] The present invention provides a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 30 parts of stearic acid, 15 parts of a catalyst, 30 parts of pentaerythritol, 8 parts of an emulsifier, 0.8 parts of a defoaming agent, 0.7 parts of a preservative and 15.5 parts of deionized water, and is characterized in that the method comprises the following specific steps:

[0033] S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add aminosulfonic acid, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0034] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in 95% by mass ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0035] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0036] Embodiment 4:

[0037] The present invention provides a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 30 parts of stearic acid, 20 parts of a catalyst, 20 parts of pentaerythritol, 8 parts of an emulsifier, 0.8 parts of a defoaming agent, 0.7 parts of a preservative and 20.5 parts of deionized water, and is characterized in that the method comprises the following specific steps:

[0038] S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add zinc sulfate, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0039] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in 95% by mass ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0040] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0041] Embodiment 5:

[0042] The present invention provides a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 20 parts of stearic acid, 10 parts of a catalyst, 40 parts of pentaerythritol, 5 parts of an emulsifier, 0.5 parts of a defoaming agent, 0.5 parts of a preservative and 24 parts of deionized water, and is characterized in that the method comprises the following specific steps:

[0043] S1: Weigh stearic acid and pentaerythritol and add them into a reactor, then add molybdic acid, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0044] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in 95% by mass ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0045] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0046] Example 6

[0047] The present invention provides a method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 40 parts of stearic acid, 10 parts of a catalyst, 20 parts of pentaerythritol, 10 parts of an emulsifier, 0.5 parts of a defoaming agent, 1 part of a preservative and 18.5 parts of deionized water, and is characterized in that the method comprises the following specific steps:

[0048] S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add 1%-1.5% by mass of a solid superacid catalyst, and heat the temperature inside the reactor to 180° C. until the solid matter in the reactor is completely melted, and then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product;

[0049] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in 95% by mass ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0050] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion;

[0051] The catalyst can also be a solid superacid catalyst, and its preparation method is as follows:

[0052] Dissolve ferric sulfate and stannous chloride in deionized water, add ammonia water while stirring to adjust the pH value to 8-9, filter and wash to remove harmful ions after 24 hours, dry at 115℃ for 12 hours, crush and sieve, soak in sulfuric acid solution for 5 minutes, filter, dry, and roast in a resistance furnace at 500-600℃ for 3 hours to obtain a solid superacid catalyst.

[0053] Comparative Example 1:

[0054] Compared with Example 1-4, the difference of this comparative example is that no catalyst is used. Other operations and parameters are the same as those shown in Example 1-6, and the specific steps are as follows:

[0055] S1: Weigh stearic acid and pentaerythritol and add them into a reactor, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, and then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated to obtain a crude product;

[0056] S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate;

[0057] S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

[0058] Conclusion: It can be seen that toluenesulfonic acid has the highest chemical activity, and the chemical conversion rate can reach 2% after 60 minutes of reaction. The chemical conversion rate of the other three agents is lower than 40%. It can be seen that p-toluenesulfonic acid is a better catalyst. Quaternary tetraol stearic acid was synthesized with p-toluenesulfonic acid as catalyst, tetraol and stearic acid as reactants, which has a good catalytic activity optimization effect on product synthesis.

[0059] Pentaerythritol and stearic acid were used as raw materials to study the synthesis and modification of pentaerythritol stearate under solvent-free conditions, and the effects of different reaction conditions on the yield were explored. This synthesis method has the following advantages, such as high catalytic yield, easy separation of products, degradable catalyst, zero VOC, no pollution, etc., and has good industrial application prospects.

[0060] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a pentaerythritol stearate emulsion, comprising the following raw material components: 20-40 parts of stearic acid, 10-20 parts of a catalyst, 20-40 parts of pentaerythritol, 5-10 parts of an emulsifier, 0.5-1 parts of a defoamer, 0.5-1 parts of a preservative and 10-50 parts of deionized water, characterized in that: The specific steps include: S1: Weigh stearic acid and pentaerythritol and add them to a reactor, then add a catalyst, and heat the temperature inside the reactor to 180°C until the solid matter in the reactor is completely melted, then use a water pump to intermittently reduce pressure and dehydrate while stirring until no water is generated, and after cooling, dissolve the product in chloroform, filter and recover the catalyst to obtain a crude product; S2: washing the crude product obtained in step S1 with a cold sodium bicarbonate solution to remove excess stearic acid, placing it in ethanol for recrystallization, and then filtering and drying to obtain pentaerythritol stearate; S3: adding the pentaerythritol stearate and emulsifier obtained in step S2 into deionized water and stirring for 50 min at a stirring speed of 2500 r / min, then adding a defoamer and a preservative and stirring for 30 min at a stirring speed of 2500 r / min to obtain a pentaerythritol stearate emulsion.

2. The method for preparing pentaerythritol stearate emulsion according to claim 1, characterized in that: The catalyst is one of toluenesulfonic acid, aluminum oxide, aminosulfonic acid, zinc sulfate and molybdic acid.

3. The preparation method of pentaerythritol stearate emulsion according to claim 1, characterized in that: The catalyst can also be a solid superacid catalyst, and its preparation method is as follows: Dissolve ferric sulfate and stannous chloride in deionized water, add ammonia water dropwise while stirring to adjust the pH value to 8-9, filter and wash to remove harmful ions after 24 hours, dry at 115°C for 12 hours, crush and sieve, soak in sulfuric acid solution for 5 minutes, filter, dry, and roast in a 500-600°C resistance furnace for 3 hours to obtain a solid superacid catalyst.

4. The method for preparing the pentaerythritol stearate emulsion according to claim 3, characterized in that: The molar ratio of ferric sulfate to stannous chloride is 3:1, and the sulfuric acid solution is 0.5 mol·L -1 .

5. The method for preparing pentaerythritol stearate emulsion according to claim 1, characterized in that: The mass percentage of ethanol in step S2 is 95%.

6. The method for preparing the pentaerythritol stearate emulsion according to claim 3, characterized in that: The mass percentage of the solid superacid catalyst is 1%-1.5%.

Citation Information

Patent Citations

  • Preparation method of pentaerythritol tristearate

    CN104529766A

  • Method for preparing pentaerythritol tristearate

    CN106966905A

  • Solid acid catalyst for catalyzing esterification reaction of pentaerythritol and stearic acid and preparation method of solid acid catalyst

    CN112973663A

  • Preparation method for synthesizing pentaerythritol stearate at low temperature

    CN117003638A

  • Improvements in or relating to the production of organic carboxylic esters of polyhydric alcohols

    GB663566A