Application of PEGDA gel microspheres in colorimetric detection of heavy metal ions in water body

By combining PEGDA gel microspheres with droplet microfluidic technology and UV curing methods, the expensive and complex problem of heavy metal ion detection in the existing technology is solved, and simple and efficient detection of Fe2+, Cu2+ and Cr6+ is achieved, which is suitable for on-site application.

CN118725174AActive Publication Date: 2024-10-01NANHU BRAIN COMPUTER CROSS RES INST
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410808768.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing heavy metal ion detection technology is expensive, complex and not suitable for on-site detection, and the coexistence detection methods of multiple metal ions are relatively limited, making it difficult to achieve simple, efficient and reliable detection.

Method used

Using PEGDA gel microspheres combined with droplet microfluidic technology and UV curing methods, a detection unit containing heavy metal ion indicators was prepared. Through the color change of the microspheres, simple, efficient and visual detection of Fe2+, Cu2+ and Cr6+ was achieved.

Benefits of technology

It achieves simple, efficient, and intuitive detection of heavy metal ions in water, has multi-channel detection capabilities for the same ions, is low-cost, simple to operate, and is suitable for on-site applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725174A_ABST
    Figure CN118725174A_ABST
Patent Text Reader

Abstract

The invention discloses an application of PEGDA gel microspheres in colorimetric detection of heavy metal ions in a water body. The PEGDA gel microspheres are doped with a heavy metal ion indicator. According to the PEGDA gel microspheres provided by the invention, simple, convenient, efficient and intuitive visual detection on heavy metal ions in a water body is realized through the color change degree and the HSB value measured by mobile phone software, and the detection limit of the PEGDA gel microspheres containing the Fe < 2 + > ( / Cu < 2 + > / Cr < 6 + >) ion indicator on Fe < 2 + > ( / Cu < 2 + > / Cr < 6 + >) ions in the water body is 5 [mu] mol / L ( / 5 [mu] mol / L).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer microspheres, and particularly relates to application of PEGDA gel microspheres in colorimetric detection of heavy metal ions in water. Background Art

[0002] Excessive levels of heavy metals in water bodies can cause serious harm to the natural environment and human health. For example, excessive iron (Fe) can lead to symptoms including cardiovascular failure, mental state changes, gastrointestinal bleeding, and liver and kidney failure; excessive copper (Cu) can affect people's skin, bones and teeth, and can cause gastrointestinal problems, kidney failure, blood cell damage and central nervous system depression, accompanied by cancer, cardiovascular disease, etc. High levels of copper can destroy the biological reprocessing system in water and reduce the self-purification capacity of natural water; chromium (Cr) is a cumulative poison and carcinogen. Frequent contact or drinking can cause abdominal discomfort or diarrhea. Once it enters the human body through breathing, it will irritate and corrode the human respiratory tract, causing pharyngitis or bronchitis, etc.

[0003] In order to avoid the harm of heavy metal ions to the environment and human body, it is of great significance to develop a heavy metal ion detection technology with high sensitivity and reliability. In addition, considering that heavy metal ions in pollutants usually coexist in multiple ways, they interfere with each other, and most detection methods focus on single ion detection, there is a strong practical demand for the development of convenient and reliable simultaneous detection technology for multiple metal ions. At present, the detection technologies for heavy metal ions at home and abroad include atomic absorption spectroscopy, atomic fluorescence spectroscopy, inductively coupled plasma emission spectroscopy, inductively coupled plasma mass spectrometry, X-ray fluorescence spectroscopy, ultraviolet visible spectrophotometry, enzyme analysis and immunoassay. However, large-scale instrumental analysis methods are not suitable for on-site detection due to their high price, high cost, and complex operation; biological analysis methods are difficult to prepare antigens and antibodies, and the test results are greatly affected by the environment, which limits their practical application. Based on these methods, high-sensitivity detection, identification and quantification of heavy metals can be achieved, but they always require the support of well-equipped laboratories and skilled operators, and may be very expensive.

[0004] Hydrogel is a polymer material with a three-dimensional network structure formed by chemical bonding or physical entanglement of high molecular polymers and using water as a dispersion medium. At present, there are many patent applications for the preparation method of hydrogel materials for heavy metal ion detection, but the general raw materials or the required supporting detection equipment are relatively expensive, or the preparation process is complicated, or the detection range is narrow, or it is not fast, simple and portable enough, which is not conducive to industrial production and further scientific research. For example, a composite hydrogel array for visual detection of metal ions and its preparation method and application disclosed in a Chinese invention patent application (CN 113667144A) is a composite hydrogel array for visual detection of metal ions: a double network structure hydrogel of sodium alginate and polyacrylamide is combined with a metal ion indicator to obtain a composite hydrogel, which is continuously arranged on a base to obtain a composite hydrogel array. And a Chinese invention patent application (CN 109012621A) discloses a heavy metal ion adsorption and detection type composite hydrogel fiber, which is prepared by melt spinning using sodium alginate, attapulgite, and carbon quantum dots to obtain a composite hydrogel. This method requires three steps of modification to obtain a composite hydrogel, and the preparation process is complicated, which is not conducive to industrial production. Therefore, it is of great significance to develop a reliable, rapid, simple, highly sensitive and highly selective analytical method. Summary of the invention

[0005] The purpose of the present invention is to provide an application of PEGDA gel microspheres in colorimetric detection of heavy metal ions in water, which can realize the detection of heavy metal ions (Fe 2+ , Cu 2+ and Cr 6+ ) is a simple, efficient and intuitive visual detection.

[0006] In order to achieve the above invention object, the present invention provides the following technical solutions:

[0007] The invention discloses an application of PEGDA gel microspheres in colorimetric detection of heavy metal ions in water. The PEGDA gel microspheres are doped with a heavy metal ion indicator.

[0008] Furthermore, the diameter of the PEGDA gel microspheres is between 300 and 650 μm.

[0009] Furthermore, the heavy metal ion indicator is Fe 2+ Indicator, Cu 2+ Indicator or Cr 6+ Indicator.

[0010] Further, the PEGDA gel microspheres have 2+ , Cu 2+ or Cr 6+ The detection limits were all 5 μmol / L.

[0011] Furthermore, the preparation method of the PEGDA gel microspheres comprises the following steps:

[0012] (1) preparing a dispersed phase solution including PEGDA and a heavy metal ion indicator solution;

[0013] (2) preparing an oil phase solution as a continuous phase solution;

[0014] (3) PEGDA gel microspheres were prepared by droplet microfluidics technology combined with UV curing technology.

[0015] In step (1), the heavy metal ion indicator solution is Fe 2+ Indicator solution, Cu 2+ Indicator solution or Cr 6+ Indicator solution, wherein:

[0016] Fe 2+ Indicator solution: an anhydrous ethanol solution containing 30-60 mg / mL o-phenanthroline;

[0017] Cu 2+ Indicator solution: chloroform solution containing 15-40 mg / mL bathocuproin powder;

[0018] Cr 6+ Indicator solution: 0.3-0.6 g of diphenylamino urea powder, 2-4 mL of acetone, 2-4 mL of deionized water and 0.1-0.3 mL of concentrated sulfuric acid.

[0019] Furthermore, in step (1), the PEGDA is PEG (400) DA, PEG (575) DA, PEG (600) DA or PEG (700) DA.

[0020] The step (1) specifically comprises: preparing a Fe-containing 2+ Dispersed phase solution of indicator solution: 0.3-1 mL of PEG (400, 575, 600, 700) DA, 0.05-0.2 mL of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone, 0.3-0.8 mL of Fe 2+ The indicator solution and 0.2-0.7 mL of deionized water were magnetically stirred for 10-30 minutes to obtain a dispersed phase solution; a Cu-containing 2+ Dispersed phase solution of indicator solution: 0.3-1 mL of PEG (400, 575, 600, 700) DA, 0.05-0.2 mL of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone, 0.3-0.8 mL of Cu 2+The indicator solution and 0.5-1.5 mL of anhydrous ethanol were magnetically stirred for 10-35 minutes to obtain a dispersed phase solution; 6+ Dispersed phase solution of indicator solution: 1.1-2 mL of PEG (400, 575, 600, 700) DA, 0.1-0.5 mL of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone and 0.3-0.8 mL of Cr in a brown glass bottle. 6+ The indicator solution is magnetically stirred for 10 to 30 minutes to obtain a dispersed phase solution.

[0021] The step (2) is specifically as follows: adding oil (silicone oil, liquid paraffin or n-hexadecane) and 1-5 wt% of a Span series surfactant into a beaker, stirring until completely dissolved, and obtaining a continuous phase solution.

[0022] Furthermore, in step (3), the continuous phase flow rate is 10-200 μL / min, the dispersed phase flow rate is 5-50 μL / min, the ratio of the dispersed phase flow rate to the continuous phase flow rate is 1:1-10, and the 365 nm ultraviolet light intensity is 30-80 mW / cm 2 , the lighting time is 1 to 15s.

[0023] The step (3) specifically comprises: setting up a droplet microfluidic platform, using a flow focusing chip with a minimum channel diameter of 200 to 500 μm, turning on a syringe pump, adjusting the syringe pump parameters so that the continuous phase flow rate is 10 to 200 μL / min, the dispersed phase flow rate is 5 to 50 μL / min, and the ratio of the dispersed phase flow rate to the continuous phase flow rate is 1:1 to 10, and after the microdroplets are stably and continuously generated, turning on a 365 nm ultraviolet lamp so that the ultraviolet light intensity received by each microdroplet is 30 to 80 mW / cm 2 , the illumination time is 1 to 15 seconds, the solidified microspheres are collected, and then washed with deionized water and anhydrous ethanol and filtered, and repeated 3 times to obtain polyethylene glycol diacrylate (PEGDA) gel microspheres doped with heavy metal ion indicators (also known as PEGDA hydrogel microspheres).

[0024] Compared with the prior art, the present invention has the following technical effects:

[0025] The PEGDA gel microspheres for colorimetric detection of heavy metal ions in water provided by the present invention are prepared by droplet microfluidics technology combined with ultraviolet light bulk polymerization. Each microsphere is a detection unit. The Fe in water is detected by measuring the color change of the microspheres and the HSB value of the mobile phone software. 2+ ( / Cu 2+ / Cr 6+ ) It can realize simple, efficient and intuitive visual detection of heavy metal ions. In addition, it can realize simultaneous multi-channel detection of the same ions and simultaneous multi-channel detection of different ions.

[0026] The PEGDA gel microsphere material provided by the present invention has high utilization rate, multiple detection units, low cost, and simple operation, and can realize visual detection of heavy metal ions anytime and anywhere, which provides a new method for simple, efficient, and intuitive detection of heavy metal ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The Fe 2+ , Cu 2+ and Cr 6+ Light microscopy images and particle size statistics of PEGDA gel microspheres as ion indicators (dispersed phase flow rate is 30 μL / min, continuous phase flow rate is 200 μL / min): (a) Fe 2+ PEGDA gel microspheres containing ion indicators, (b) Cu 2+ PEGDA gel microspheres containing ion indicators, (c) Cr 6+ PEGDA gel microspheres as ion indicators.

[0028] Figure 2 is the dispersed phase flow rate and Fe content in Examples 1-3 2+ , Cu 2+ Cr 6+ Size relationship diagram of PEGDA gel microspheres of ion indicators (continuous phase flow rate is 200 μL / min).

[0029] Figure 3 The Fe content in Examples 1-3 2+ , Cu 2+ and Cr 6+ PEGDA gel microspheres with ion indicators were used to detect Fe 2 + , Cu 2+ and Cr 6+ SEM images ((a), (b), (c)) and EDS images ((d), (e), (f)) after ion solution.

[0030] Figure 4 Colorimetric analysis of PEGDA gel microspheres showing different concentrations of heavy metal ions: (a) Fe 2+ (b) Cu 2+ and (c)Cr 6+ .

[0031] Figure 5 The relationship between the measured HSB value of the PEGDA gel microsphere color and the concentration of each heavy metal ion is shown in the figure: (a) Fe 2+ (b) Cu 2+ and (c)Cr 6+ .

[0032] Figure 6 Colorimetric analysis of PEGDA films showing different concentrations of heavy metal ions: (d) Fe 2+ 、(e)Cu 2+ and (f)Cr 6 + . DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the embodiments and drawings. It is necessary to point out that the following embodiments are only used to explain and illustrate the present invention and are not used to limit the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above invention content still belong to the protection scope of the present invention.

[0034] The application method of the PEGDA gel microspheres doped with a heavy metal ion indicator provided by the present invention in the colorimetric detection of heavy metal ions in water is as follows:

[0035] The PEGDA gel microspheres were evenly spread in each cylindrical pit in the mold. As a comparative example, the above dispersed phase solution was dripped into each cylindrical pit, and then the ultraviolet light intensity of the ultraviolet lamp at 365nm was 30-80mW / cm 2 , the illumination time is 1 to 15 seconds, and a polyethylene glycol diacrylate (PEGDA) hydrogel film doped with a heavy metal ion indicator is obtained.

[0036] Prepare Fe-containing solutions with concentrations of 0, 5, 10, 15, 20, 40, 80, 100, 300, and 500 μmol / L. 2+ (FeCl2){ / Cu 2+ (CuSO4) / Cr 6+ (K2Cr2O7)} test solution, and then use a pipette to absorb the Fe 2+ (FeCl2){ / Cu 2+ (CuSO4) / Cr 6+ A drop of the solution to be tested (K2Cr2O7) was dripped into each cylindrical pit in the mold. After a few seconds, the Fe 2+ ( / Cu 2+ / Cr 6+ ) The polyethylene glycol diacrylate (PEGDA) hydrogel microspheres and films, which are heavy metal ion indicators, change from colorless to red (yellow / purple), and then the HSB value is measured by the color change degree of the microspheres and films and the mobile phone software.

[0037] Example 1

[0038] In this embodiment, a colorimetric method for detecting Fe in water was prepared based on droplet microfluidics technology. 2+ The detailed process of PEGDA gel microspheres with heavy metal ions is as follows:

[0039] (1) Preparation of dispersed phase solution: Preparation of Fe 2+ Indicator solution: add 0.3 g of white o-phenanthroline powder and 6 mL of anhydrous ethanol to a glass bottle and stir magnetically for 10 minutes until the solution is clear. Then add 0.5 mL of PEG (400) DA, 0.1 mL of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone, 0.5 mL of Fe 2+ The indicator solution and 0.5 mL of deionized water were magnetically stirred for 10 min to obtain a dispersed phase solution.

[0040] (2) Preparation of continuous phase solution: Add liquid paraffin and 2 wt % Span 80 surfactant into a beaker and stir until completely dissolved to obtain a continuous phase solution.

[0041] (3) Preparation of PEGDA gel microspheres by droplet microfluidics combined with UV curing technology: Set up the droplet microfluidics platform, use a flow focusing chip with a minimum channel diameter of 200 μm, turn on the syringe pump, adjust the syringe pump parameters to make the continuous phase flow rate 200 μL / min, and the dispersed phase flow rate 30 μL / min, and after the microdroplets are stably and continuously generated, turn on the 365 nm UV lamp so that each microdroplet is exposed to a UV light intensity of 30 mW / cm 2 The solidified microspheres were collected, washed with deionized water and anhydrous ethanol, and filtered. This was repeated three times to obtain Fe-doped microspheres. 2+ Polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator.

[0042] The Fe-doped 2+ The heavy metal ion indicator polyethylene glycol diacrylate (PEGDA) hydrogel microspheres are evenly spread on the Figure 4 In each cylindrical pit in the mold shown in (a). Figure 6 Each cylindrical pit in the mold shown in (d) is filled with the above dispersed phase solution, and then the ultraviolet light intensity of 365nm ultraviolet lamp is 30mW / cm 2 , the illumination time is 5s, and Fe-doped 2+ Then, the concentrations of 0, 5, 10, 15, 20, 40, 80, 100, 300, and 500 μmol / L of Fe-containing 2+ (FeCl2) test solution, and then use a pipette to absorb the Fe2+ A drop of the test solution (FeCl2) was dripped into each cylindrical pit in the mold. After a few seconds, the Fe 2+ The polyethylene glycol diacrylate (PEGDA) hydrogel microspheres and films of heavy metal ion indicator changed from colorless to red, and then the HSB value was measured by the color change degree of the microspheres and films and the mobile phone software.

[0043] The obtained Fe-doped 2+ The optical micrograph and particle size statistics of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator are shown in Figure 1 As shown in (a), the dispersed phase flow rate and Fe content 2+ The size relationship diagram of PEGDA gel microspheres of ion indicators (continuous phase flow rate is 200μL / min) is shown in Figure 2 As shown, the Fe-doped 2+ The scanning electron microscope (SEM) image of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator is shown in Figure 3 As shown in (a) and the energy spectrum (EDS) diagram is as follows Figure 3 As shown in (d), Fe 2+ PEGD A gel microsphere colorimetric analysis of heavy metal ion indicators shows different concentrations of Fe 2+ Heavy metal ions such as Figure 4 As shown in (a), according to the measured Fe-doped 2+ The HSB value of the color of PEGDA gel microspheres as heavy metal ion indicator and Fe 2+ The relationship between heavy metal ion concentration and Figure 5 As shown in (a), Fe 2+ PEGDA film colorimetric analysis of heavy metal ion indicators showing different concentrations of Fe 2+ Heavy metal ions such as Figure 6 As shown in (d) in .

[0044] In this embodiment, about 95% of the Fe-doped 2+ The particle size of the polyethylene glycol diacrylate (PEGDA) hydrogel microspheres of the heavy metal ion indicator is 365-405 μm. When the dispersed phase flow rate changes from 5 to 50 μL / min, the microsphere particle size is 60-650 μm (the continuous phase flow rate is 200 μL / min). 2+ PEGDA film as heavy metal ion indicator for Fe 2+ The detection limit of the solution doped with FeCl2 was 80 μmol / L. 2+ PEGDA gel microspheres as heavy metal ion indicator for Fe 2+The detection limit of the test solution is 5 μmol / L. 2+ As the concentration of the (FeCl2) test solution increases, the color of the microspheres becomes increasingly red.

[0045] Example 2

[0046] In this embodiment, a colorimetric method for detecting Cu in water was prepared based on droplet microfluidics technology. 2+ The detailed process of PEGDA gel microspheres with heavy metal ions is as follows:

[0047] (1) Preparation of dispersed phase solution: Preparation of Cu 2+ Indicator solution: add 0.15g of bathocuproin powder and 6mL of chloroform into a glass bottle and stir magnetically for 20 minutes until the solution is clear. Then add 0.5mL of PEG(400)DA, 0.1mL of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone, 0.5mL of Cu 2+ The indicator solution and 0.5 mL of anhydrous ethanol were magnetically stirred for 15 min to obtain a dispersed phase solution.

[0048] (2) Preparation of continuous phase solution: Add liquid paraffin and 2 wt % Span 80 surfactant into a beaker and stir until completely dissolved to obtain a continuous phase solution.

[0049] (3) Preparation of PEGDA gel microspheres by droplet microfluidics combined with UV curing technology: Set up the droplet microfluidics platform, use a flow focusing chip with a minimum channel diameter of 200 μm, turn on the syringe pump, adjust the syringe pump parameters to make the continuous phase flow rate 200 μL / min, and the dispersed phase flow rate 30 μL / min, and after the microdroplets are stably and continuously generated, turn on the 365 nm UV lamp so that each microdroplet is exposed to a UV light intensity of 30 mW / cm 2 The solidified microspheres were collected, washed with deionized water and anhydrous ethanol, and filtered. This was repeated three times to obtain Cu-doped microspheres. 2+ Polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator.

[0050] The Cu-doped 2+ The heavy metal ion indicator polyethylene glycol diacrylate (PEGDA) hydrogel microspheres are evenly spread on the Figure 4 In each cylindrical pit in the mold shown in (b). Figure 6 Each cylindrical pit in the mold shown in (e) is filled with the dispersed phase solution, and then the ultraviolet light intensity of the ultraviolet lamp at 365nm is 30mW / cm 2 , the illumination time is 5s, and Cu 2+Then, the concentrations of 0, 5, 10, 15, 20, 40, 80, 100, 300, and 500 μmol / L containing Cu were prepared. 2+ (CuSO4) test solution, and then use a pipette to absorb the Cu 2+ A drop of the test solution (CuSO4) was dripped into each cylindrical pit in the mold. After a few seconds, the solution doped with Cu 2+ The polyethylene glycol diacrylate (PEGDA) hydrogel microspheres and films of the heavy metal ion indicator changed from colorless to yellow, and then the HSB value was measured by the color change degree of the microspheres and films and the mobile phone software.

[0051] The obtained Cu-doped 2+ The optical micrograph and particle size statistics of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator are shown in Figure 1 As shown in (b), the dispersed phase flow rate and Cu content 2+ The size relationship diagram of PEGDA gel microspheres of ion indicators (continuous phase flow rate is 200μL / min) is shown in Figure 2 As shown, the Cu-doped 2+ The scanning electron microscope (SEM) image of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator is shown in Figure 3 As shown in (b), the energy spectrum (EDS) is as follows Figure 3 As shown in (e), Cu 2+ PEGD A gel microsphere colorimetric analysis of heavy metal ion indicators shows different concentrations of Cu 2+ Heavy metal ions such as Figure 4 As shown in (b), according to the measured Cu-doped 2+ The HSB value of the color of PEGDA gel microspheres as heavy metal ion indicator and Cu 2+ The relationship between heavy metal ion concentration and Figure 5 As shown in (b), Cu 2+ PEGDA film colorimetric analysis of heavy metal ion indicators shows different concentrations of Cu 2+ Heavy metal ions such as Figure 6 As shown in (e) in .

[0052] About 90% of the Cu-doped 2+ The particle size of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres of heavy metal ion indicator is 340-400 μm. When the dispersed phase flow rate changes from 5-50 μL / min, the microsphere particle size is 70-650 μm (the continuous phase flow rate is 200 μL / min). 2+PEGDA film as heavy metal ion indicator for Cu 2+ The detection limit of the solution doped with CuSO4 was 15 μmol / L. 2+ Heavy metal ion indicator PEGDA gel microspheres for Cu 2+ The detection limit of the solution containing CuSO4 is 5 μmol / L. 2+ As the concentration of the (CuSO4) test solution increases, the color of the microspheres becomes increasingly yellow.

[0053] Example 3

[0054] In this embodiment, a colorimetric method for detecting Cr in water is prepared based on droplet microfluidics technology. 6+ The detailed process of PEGDA gel microspheres with heavy metal ions is as follows:

[0055] (1) Preparation of dispersed phase solution: Preparation of Cr 6+ Indicator solution: 0.36 g of diphenylamino urea powder, 3 mL of acetone, 3 mL of deionized water, and 0.2 mL of concentrated sulfuric acid were added to a glass bottle and stirred magnetically for 30 minutes until the solution was clear. Then 1.5 mL of PEG (400) DA, 0.3 mL of photoinitiator 2-hydroxy-2-methyl-1-phenylpropanone, and 0.5 mL of Cr were added to a brown glass bottle. 6+ The indicator solution was stirred magnetically for 10 minutes to obtain a dispersed phase solution.

[0056] (2) Preparation of continuous phase solution: Add liquid paraffin and 2 wt % Span 80 surfactant into a beaker and stir until completely dissolved to obtain a continuous phase solution.

[0057] (3) Preparation of PEGDA gel microspheres by droplet microfluidics combined with UV curing technology: Set up the droplet microfluidics platform, use a flow focusing chip with a minimum channel diameter of 200 μm, turn on the syringe pump, adjust the syringe pump parameters to make the continuous phase flow rate 200 μL / min, and the dispersed phase flow rate 30 μL / min, and after the microdroplets are stably and continuously generated, turn on the 365 nm UV lamp so that each microdroplet is exposed to a UV light intensity of 30 mW / cm 2 The solidified microspheres were collected, washed with deionized water and anhydrous ethanol, and filtered. This was repeated three times to obtain the Cr-doped microspheres. 6+ Polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator.

[0058] The Cr-doped 6+ The heavy metal ion indicator polyethylene glycol diacrylate (PEGDA) hydrogel microspheres are evenly spread on the Figure 4In each cylindrical pit in the mold shown in (c). Figure 6 Each cylindrical pit in the mold shown in (f) is filled with the above dispersed phase solution, and then the ultraviolet light intensity of the ultraviolet lamp at 365nm is 30mW / cm 2 , the illumination time is 2s, and Cr-doped 6+ Then, 0, 5, 10, 15, 20, 40, 80, 100, 300, and 500 μmol / L of Cr-containing 6+ (K2Cr2O7) solution to be tested, and then use a pipette to absorb the Cr 6+ A drop of the test solution (K2Cr2O7) was dripped into each cylindrical pit in the mold. After a few seconds, the Cr-doped 6+ The polyethylene glycol diacrylate (PEGDA) hydrogel microspheres and films of the heavy metal ion indicator changed from colorless to purple, and then the HSB value was measured by the color change degree of the microspheres and films and the mobile phone software.

[0059] The obtained Cr-doped 6+ The optical micrograph and particle size statistics of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator are shown in Figure 1 As shown in (c), the dispersed phase flow rate and Cr content 6+ The size relationship diagram of PEGDA gel microspheres of ion indicators (continuous phase flow rate is 200μL / min) is shown in Figure 2 As shown, the Cr-doped 6+ The scanning electron microscope (SEM) image of polyethylene glycol diacrylate (PEGDA) hydrogel microspheres as heavy metal ion indicator is shown in Figure 3 As shown in (c) in the figure, the energy spectrum (EDS) is as follows Figure 3 As shown in (f), Cr 6+ The heavy metal ion indicator PEGD A gel microsphere colorimetric analysis showed different concentrations of Cr 6+ Heavy metal ions such as Figure 4 As shown in (c), according to the measured Cr-doped 6+ The HSB value of the color of PEGDA gel microspheres as heavy metal ion indicator and Cr 6+ The relationship between heavy metal ion concentration and Figure 5 As shown in (c), Cr 6+ Colorimetric analysis of PEGDA thin films as heavy metal ion indicators showing different concentrations of Cr 6+ Heavy metal ions such as Figure 6 As shown in (f) in .

[0060] About 90% of the Cr-doped6+ The particle size of the polyethylene glycol diacrylate (PEGDA) hydrogel microspheres of the heavy metal ion indicator is 360-400 μm. When the dispersed phase flow rate changes from 5 to 50 μL / min, the microsphere particle size is 75-650 μm (the continuous phase flow rate is 200 μL / min). 6+ PEGDA film as heavy metal ion indicator for Cr-containing 6+ The detection limit of the solution doped with Cr was 15 μmol / L. 6+ PEGDA gel microspheres as heavy metal ion indicator for Cr-containing 6+ The detection limit of the solution containing Cr is 5 μmol / L. 6+ As the concentration of the (K2Cr2O7) test solution increases, the color of the microspheres becomes increasingly purple.

[0061] In summary, the Fe-containing 2+ ( / Cu 2+ / Cr 6+ ) ion indicator PEGDA gel microspheres for Fe in water 2+ ( / Cu 2+ / Cr 6+ ) ions have a detection limit of 5 μmol / L ( / 5 μmol / L / 5 μmol / L), while Fe 2+ ( / Cu 2+ / Cr 6+ ) PEGDA film as an ion indicator for Fe in water 2+ ( / Cu 2+ / Cr 6+ ) ions have a detection limit of 80μmol / L ( / 15μmol / L / 15μmol / L). Since the microspheres are uniform in size and small in diameter, their spherical structure has an amplifying effect on color. Compared with thin films, gel microspheres show better detection performance and can improve the detection signal of heavy metal ions.

Claims

1. Application of PEGDA gel microspheres in colorimetric detection of heavy metal ions in water, characterized in that: The PEGDA gel microspheres are doped with a heavy metal ion indicator.

2. The use according to claim 1, characterized in that: The diameter of the PEGDA gel microspheres is 300-650 μm.

3. The use according to claim 1, characterized in that: The heavy metal ion indicator is Fe 2+ Indicator, Cu 2+ Indicator or Cr 6+ Indicator.

4. The use according to claim 3, characterized in that: The PEGDA gel microspheres have 2+ , Cu 2+ or Cr 6+ The detection limits were all 5 μmol / L.

5. The use according to any one of claims 1 to 4, characterized in that: The preparation method of the PEGDA gel microspheres comprises the following steps: (1) preparing a dispersed phase solution including PEGDA and a heavy metal ion indicator solution; (2) preparing an oil phase solution as a continuous phase solution; (3) PEGDA gel microspheres were prepared by droplet microfluidics technology combined with UV curing technology.

6. The use according to claim 5, characterized in that: In step (1), the heavy metal ion indicator solution is Fe 2+ Indicator solution, Cu 2+ Indicator solution or Cr 6+ Indicator solution, wherein: Fe 2+ Indicator solution: an anhydrous ethanol solution containing 30-60 mg / mL o-phenanthroline; Cu 2+ Indicator solution: chloroform solution containing 15-40 mg / mL bathocuproin powder; Cr 6+ Indicator solution: 0.3-0.6 g of diphenylamino urea powder, 2-4 mL of acetone, 2-4 mL of deionized water and 0.1-0.3 mL of concentrated sulfuric acid.

7. The use according to claim 5, characterized in that: In step (1), the PEGDA is PEG (400) DA, PEG (575) DA, PEG (600) DA or PEG (700) DA.

8. The use according to claim 5, characterized in that: In step (3), the continuous phase flow rate is 10-200 μL / min, the dispersed phase flow rate is 5-50 μL / min, the ratio of the dispersed phase flow rate to the continuous phase flow rate is 1:1-10, and the 365 nm ultraviolet light intensity is 30-80 mW / cm 2 , the lighting time is 1 to 15s.

9. The use according to any one of claims 1 to 4, characterized in that: The PEGDA gel microspheres can realize visual detection of heavy metal ions in water by measuring the degree of color change and HSB value using mobile phone software.

Citation Information

Patent Citations

  • Smartphone-based apparatus and method for obtaining repeatable, quantitative colorimetric measurement

    CN105164514A

  • Method for rapid and accurate colorimetric detection of heavy metal ions

    CN112540078A

  • Composite hydrogel array for visually detecting metal ions, and preparation method and application thereof

    CN113667144A

  • Hydrogel hollow microsphere preparation method based on micro-fluidic controllable photocuring technology and product and application thereof

    CN117504749A

  • A nanoparticle based chromogenic regent and preparation method, methods and kits for semi-quantitative detection of iron fortified rice or cereals