Temperature-resistant polyacrylamide resistance reducing agent as well as preparation method and application thereof
By copolymerizing sodium fluorine-containing acrylate sulfonate and acrylamide, a temperature-resistant polyacrylamide resistance reducing agent with a disulfonate group and a double perfluorocarbon chain structure is formed, which solves the problem of temperature resistance, salt resistance and shear resistance. Solve the problem of insufficient performance and achieve efficient resistance reduction in shale gas development.
Patent Information
- Application Number
- CN202410933005.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
AI Technical Summary
Polyacrylamide resistance reducing agent has poor temperature resistance, salt resistance and shear resistance, which affects its application in shale gas development.
Fluorine-containing sodium acrylate sulfonate is used as the functional monomer to copolymerize with acrylamide to form a temperature-resistant polyacrylamide resistance reducing agent with a disulfonate group and a dual perfluorocarbon chain structure. It is combined with a surfactant and uses a specific The preparation method improves its heat resistance and shear resistance.
Significantly improves the temperature resistance and shear resistance of polyacrylamide resistance reducing agent, the resistance reduction rate reaches 68.7-77.3%, shows excellent resistance reduction effect in high temperature and high salt environment, and is suitable for shale gas reservoirs fracturing technology.
Smart Images

Figure BDA0004940404500000022 
Figure BDA0004940404500000031 
Figure BDA0004940404500000032
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fracturing drag reducing agents, and in particular relates to a temperature-resistant polyacrylamide drag reducing agent and a preparation method and application thereof. Background Art
[0002] Slickwater fracturing technology is widely used in shale gas development and other fields. The fracturing fluid mainly contains surfactants, drag reducers, clay stabilizers and other additives. Among them, drag reducers have a great influence on the performance of fracturing fluid. When slickwater fracturing fluid is pumped into the formation at high speed through the pipe string, there is a large friction resistance between the fracturing fluid and the pipe wall, which will increase energy loss. Therefore, the development of high-performance drag reducers is a research hotspot. Drag reducers mainly include polyacrylamide, guar gum derivatives, viscoelastic surfactants and other drag reducers.
[0003] Polyacrylamide has low cost, simple preparation, good drag reduction effect, and has achieved good practical application. However, the shear resistance of polyacrylamide drag reducer is poor, and the molecular chain is easy to break, resulting in a decrease in the molecular weight of the polymer, which will affect its drag reduction effect. The development of heat-resistant, salt-resistant, and shear-resistant polyacrylamide drag reducer is a research hotspot. Usually, functional monomers such as N-vinyl pyrrolidone, sodium styrene sulfonate, 2-acrylamido-2-methylpropyl sulfonic acid, etc. are used to copolymerize with acrylamide to improve the heat resistance and salt resistance of polyacrylamide drag reducer. Summary of the invention
[0004] The invention solves the problem that the polyacrylamide resistance reducing agent has poor performances such as temperature resistance and salt resistance.
[0005] Technical solution: A heat-resistant polyacrylamide drag reducing agent comprises the following raw materials: acrylamide, sodium fluorinated acrylate sulfonate, azobisisobutyramidine hydrochloride, and a surfactant in a molar ratio of (94-99):(1-6):(0.06-0.075).
[0006] Fluorinated sodium acrylamide sulfonate has the structural formula (1):
[0007] Where n is 5, 6 or 7.
[0008] Preferably, the surfactant is sodium dodecyl sulfate or sodium dodecylbenzene sulfonate.
[0009] Preferably, the preparation method of the heat-resistant polyacrylamide drag reducing agent is as follows: acrylamide, sodium fluorinated acrylate sulfonate, and a surfactant are added to deionized water, stirred and mixed, and then heated to the reaction temperature, azobisisobutylamidine hydrochloride is added in a nitrogen atmosphere, ethanol is added after the reaction to precipitate, filtered, washed with ethanol, and dried to obtain the heat-resistant polyacrylamide drag reducing agent.
[0010] Preferably, the reaction temperature is 50-65°C and the reaction time is 4-8h.
[0011] Preferably, the preparation method of fluorinated sodium acrylate sulfonate is:
[0012] S1. Add 1,7-bis-BOC-1,4,7-triazaheptane, 2-bromoethyl acrylate and potassium carbonate in a molar ratio of 1:(1-1.2):(1.8-2.5) to acetonitrile, heat to 40-70°C, filter after cooling, and perform rotary evaporation on the filtrate. Then, dissolve the product in dichloromethane and trifluoroacetic acid, stir and react for 3-4h, perform rotary evaporation, add saturated sodium bicarbonate and ethyl acetate, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, and rotary evaporate the filtrate to obtain intermediate 1. The reaction formula is as follows:
[0013]
[0014] S2. Add deionized water, sodium hydroxide, and intermediate 1 to 1,4-dioxane, mix well, and add 1,4-butane sultone, wherein the molar ratio of sodium hydroxide, intermediate 1, and 1,4-butane sultone is (2-2.2):1:(2-2.2), heat to 65-75°C, react for 5-8h, add hydrochloric acid to adjust the pH of the solution to neutral, filter, rotary evaporate the filtrate, and dry to obtain intermediate 2. The reaction formula is:
[0015]
[0016] S3, add intermediate 2 in a molar ratio of 1:(2.2-2.6):(2.3-2.8) to chloroform,
[0017] Perfluoroacyl chloride compound and triethylamine, react at room temperature for 24-36 hours, add deionized water, extract and separate.
[0018] The organic phase was dried over anhydrous sodium sulfate, filtered, and the filtrate was rotary evaporated and dried to obtain fluorinated acrylic acid.
[0019] Sodium ester sulfonate. The reaction formula is:
[0020]
[0021] Preferably, the structural formula of the perfluoroacyl chloride compound is Where n is 5, 6 or 7
[0022] Preferably, the heat-resistant polyacrylamide drag reducing agent is used as a drag reducing agent for fracturing fluid.
[0023] The technical effect is: the present invention uses fluorinated sodium acrylate sulfonate as a functional monomer and propylene
[0024] The heat-resistant polyacrylamide drag reducing agent obtained by amide polymerization contains disulfonate groups and diperfluoro
[0025] Carbon chain structure, sulfonate can provide negative charge to the polyacrylamide molecular chain and form a larger side
[0026] The base has a larger hydrodynamic volume, which can make the polyacrylamide molecular chain less likely to curl up.
[0027] It exhibits excellent salt resistance and shear resistance.
[0028] The perfluorocarbon chain group contained in the fluorinated sodium acrylate sulfonate of the present invention has strong thermal stability, can improve the heat resistance of polyacrylamide, the molecular chain is not easy to decompose at high temperature, and a strong hydrophobic association can be formed between the perfluorocarbon chain groups, which can further improve the shear resistance of the drag reducing agent. The drag reduction rate of the heat-resistant polyacrylamide drag reducing agent prepared by the present invention reaches 68.7-77.3%, the drag reduction effect is good, and it has good practical application in the fracturing technology of shale gas reservoirs. DETAILED DESCRIPTION
[0029] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.
[0030] Example 1
[0031] S1. Add 4 mmol 1,7-bis-BOC-1,4,7-triazaheptane (CAS No. 117499-16-8), 4.4 mmol 2-bromoethyl acrylate (CAS No. 4823-47-6), and 7.2 mmol potassium carbonate to 15 mL acetonitrile, heat to 50°C, filter after cooling, and rotary evaporate the filtrate. Then dissolve the product in 6 mL dichloromethane and 4 mL trifluoroacetic acid, stir and react for 4 h, rotary evaporate, add saturated sodium bicarbonate and ethyl acetate, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain intermediate 1.
[0032] S2. Add 5 mL of deionized water, 8.8 mmol of sodium hydroxide and 4 mmol of intermediate 1 to 4 mL of 1,4-dioxane, mix well, add 8 mmol of 1,4-butane sultone (CAS No. 1633-83-6), heat to 65°C, react for 6 hours, add hydrochloric acid to adjust the pH of the solution to neutral, filter, rotary evaporate the filtrate, dry to remove water, wash with saturated sodium bicarbonate solution, and recrystallize with ethanol to obtain intermediate 2.
[0033] S3. Add 3 mmol of intermediate 2, 7.8 mmol of undecylfluorohexanoyl chloride (CAS No. 335-53-5) and 8.4 mmol of triethylamine to 35 mL of chloroform, react at room temperature for 24 hours, add deionized water, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain sodium fluorinated acrylate sulfonate.
[0034] S4. Add 99 mmol acrylamide, 1 mmol sodium fluorinated acrylate sulfonate, and 0.04 g surfactant sodium dodecyl sulfate to 25 mL deionized water, stir and mix, then heat to 55°C, add 0.06 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 4 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0035] Example 2
[0036] S1. Add 4 mmol 1,7-bis-BOC-1,4,7-triazaheptane, 4 mmol 2-bromoethyl acrylate and 10 mmol potassium carbonate to 10 mL acetonitrile, heat to 40°C, filter after cooling, and rotary evaporate the filtrate. Then dissolve the product in 6 mL dichloromethane and 4 mL trifluoroacetic acid, stir and react for 4 h, rotary evaporate, add saturated sodium bicarbonate and ethyl acetate, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain intermediate 1.
[0037] S2. Add 5 mL of deionized water, 8.8 mmol of sodium hydroxide and 4 mmol of intermediate 1 to 6 mL of 1,4-dioxane, mix well and add 8 mmol of 1,4-butane sultone, heat to 70 ° C, react for 5 hours, add hydrochloric acid to adjust the pH of the solution to neutral, filter and rotary evaporate the filtrate, dry to remove water, wash with saturated sodium bicarbonate solution, and recrystallize with ethanol to obtain intermediate 2.
[0038] S3. Add 3 mmol of intermediate 2, 6.6 mmol of tridecafluoroheptanoyl chloride (CAS No. 52447-22-0) and 8.4 mmol of triethylamine to 25 mL of chloroform, react at room temperature for 36 hours, add deionized water, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain sodium fluorinated acrylate sulfonate.
[0039] S4. Add 97.5 mmol acrylamide, 2.5 mmol sodium fluorinated acrylate sulfonate, and 0.1 g of surfactant sodium dodecylbenzene sulfonate to 25 mL of deionized water, stir and mix, then heat to 50°C, add 0.065 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 8 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0040] Example 3
[0041] S1. Add 4 mmol 1,7-bis-BOC-1,4,7-triazaheptane, 4.8 mmol 2-bromoethyl acrylate and 8.5 mmol potassium carbonate to 12 mL acetonitrile, heat to 40°C, filter after cooling, and rotary evaporate the filtrate. Then dissolve the product in 6 mL dichloromethane and 4 mL trifluoroacetic acid, stir and react for 3 h, rotary evaporate, add saturated sodium bicarbonate and ethyl acetate, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain intermediate 1.
[0042] S2. Add 5 mL of deionized water, 8 mmol of sodium hydroxide and 4 mmol of intermediate 1 to 4 mL of 1,4-dioxane, mix well and add 8 mmol of 1,4-butane sultone, heat to 75°C, react for 5 h, add hydrochloric acid to adjust the pH of the solution to neutral, filter and rotary evaporate the filtrate, dry to remove water, wash with saturated sodium bicarbonate solution, and recrystallize with ethanol to obtain intermediate 2.
[0043] S3. Add 3 mmol of intermediate 2, 7.2 mmol of tridecafluoroheptanoyl chloride (CAS No. 52447-22-0) and 8.4 mmol of triethylamine to 30 mL of chloroform, react at room temperature for 36 hours, add deionized water, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain sodium fluorinated acrylate sulfonate.
[0044] S4. Add 96 mmol acrylamide, 4 mmol sodium fluorinated acrylate sulfonate, and 0.18 g of surfactant sodium dodecyl sulfate to 30 mL of deionized water, stir and mix, then heat to 65°C, add 0.075 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 4 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0045] Example 4
[0046] S1. Add 4 mmol 1,7-bis-BOC-1,4,7-triazaheptane, 4 mmol 2-bromoethyl acrylate and 7.2 mmol potassium carbonate to 10 mL acetonitrile, heat to 70°C, filter after cooling, and rotary evaporate the filtrate. Then dissolve the product in 7 mL dichloromethane and 5 mL trifluoroacetic acid, stir and react for 3 h, rotary evaporate, add saturated sodium bicarbonate and ethyl acetate, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain intermediate 1.
[0047] S2. Add 6 mL of deionized water, 8.4 mmol of sodium hydroxide and 4 mmol of intermediate 1 to 5 mL of 1,4-dioxane, mix well and add 8.8 mmol of 1,4-butane sultone, heat to 65 ° C, react for 8 hours, add hydrochloric acid to adjust the pH of the solution to neutral, filter and rotary evaporate the filtrate, dry to remove water, wash with saturated sodium bicarbonate solution, and recrystallize with ethanol to obtain intermediate 2.
[0048] S3. Add 3 mmol of intermediate 2, 6.6 mmol of perfluorooctanoyl chloride (CAS No. 335-66-0) and 7.2 mmol of triethylamine to 35 mL of chloroform, react at room temperature for 36 hours, add deionized water, extract and separate, dry the organic phase with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, and dry to obtain sodium fluorinated acrylate sulfonate.
[0049] S4. Add 94 mmol acrylamide, 6 mmol sodium fluorinated acrylate sulfonate, and 0.25 g of surfactant sodium dodecylbenzene sulfonate to 30 mL of deionized water, stir and mix, then heat to 65 ° C, add 0.075 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 6 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0050] Comparative Example 1
[0051] The difference between this comparative example and Example 1 is that no fluorinated sodium acrylate sulfonate is added.
[0052] S1. Add 99 mmol acrylamide and 0.04 g surfactant sodium dodecyl sulfate to 25 mL deionized water, stir and mix well, then heat to 55 °C, add 0.06 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 4 h, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0053] Comparative Example 2
[0054] The difference between this comparative example and Example 1 is that 2-acrylamido-2-methylpropyl sulfonic acid (CAS No. 15214-89-8) is used instead of fluorinated sodium acrylate sulfonate.
[0055] S4. Add 99 mmol acrylamide, 1 mmol sodium 2-acrylamido-2-methylpropyl sulfonate, and 0.04 g of surfactant sodium dodecyl sulfate to 25 mL of deionized water, stir and mix, then heat to 55°C, add 0.06 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 4 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0056] Comparative Example 3
[0057] The difference between this comparative example and Example 1 is that dodecafluoroheptyl methacrylate (CAS No. 2261-99-6) is used instead of sodium fluorinated acrylate sulfonate.
[0058] S4. Add 99 mmol acrylamide, 1 mmol dodecafluoroheptyl methacrylate, and 0.04 g of surfactant sodium dodecyl sulfate to 25 mL of deionized water, stir and mix, then heat to 55°C, add 0.06 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 4 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0059] Comparative Example 4
[0060] The difference between this comparative example and Example 1 is that dodecafluoroheptyl methacrylate (0.5 mmol) and sodium 2-acrylamido-2-methylpropyl sulfonate (0.5 mmol) are used instead of sodium fluorine-containing acrylate sulfonate (1 mmol).
[0061] To 25 mL of deionized water, add 99 mmol acrylamide, 0.5 mmol sodium 2-acrylamido-2-methylpropyl sulfonate, 0.5 mmol dodecafluoroheptyl methacrylate, and 0.04 g of surfactant sodium dodecyl sulfate, stir and mix well, then heat to 55 ° C, add 0.06 mmol azobisisobutylamidine hydrochloride in a nitrogen atmosphere, react for 4 hours, add ethanol to precipitate, filter, wash with ethanol and dry to obtain a heat-resistant polyacrylamide drag reducer.
[0062] Add polyacrylamide drag reducing agent to deionized water to prepare a 0.3% solution, and use a rotational viscometer to test the apparent viscosity of the solution. The test temperature is 25-140℃, and the shear rate is 170s- 1 . The shearing time is 20min.
[0063] Table 1 Apparent viscosity of polyacrylamide drag reducing agent at different temperatures
[0064]
[0065]
[0066] Sodium chloride, potassium chloride, calcium chloride, and magnesium chloride were added to deionized water to control the mineralization of the solution to 5000-20000 mg / L, and polyacrylamide drag reducer was added to control the mass fraction of polyacrylamide drag reducer in the solution to 0.3%. The apparent viscosity of the solution was tested using a rotational viscometer. The test temperature was 25°C, and the shear rate was 170s- 1 . The shearing time is 20 minutes.
[0067] Table 2 Apparent viscosity of polyacrylamide drag reducing agent at different mineralization degrees
[0068]
[0069] After testing, the apparent viscosity of the heat-resistant polyacrylamide drag reducing agent of Examples 1-4 at 25°C reached 38.0-52.3 mPa·s. And at a high temperature of 140°C, the apparent viscosity still reached 35.9-47.7 mPa·s, and in a high-salt and high-mineralization system of 15000 mg / L, the apparent viscosity remained at 27.4-36.9 mPa·s.
[0070] Taking Example 1 as an example, its high temperature apparent viscosity retention rate reaches 87.68% (36.3 / 41.4). The high salt apparent viscosity retention rate reaches 68.84% (28.5 / 41.4). It shows excellent temperature resistance, salt resistance and shear resistance. This is because the heat-resistant polyacrylamide drag-reducing agent obtained by the polymerization reaction of fluorinated sodium acrylate sulfonate and acrylamide contains a disulfonate group and a di-perfluorocarbon chain structure. The sulfonate can provide a negative charge for the polyacrylamide molecular chain, has a larger hydrodynamic volume, and can make the polyacrylamide molecular chain less likely to curl, thereby showing excellent salt resistance and shear resistance. And the perfluorocarbon chain group has a strong thermal stability, which can improve the heat resistance of polyacrylamide, the molecular chain is not easy to decompose at high temperature, and a strong hydrophobic association can be formed between the perfluorocarbon chain groups, which can further improve the shear resistance of the drag-reducing agent.
[0071] In Comparative Example 1, no fluorinated sodium acrylate sulfonate was added, and the obtained polyacrylamide drag reducing agent did not contain sulfonic acid groups and perfluorocarbon chain groups, had a low apparent viscosity, and under high temperature, high salt and high mineralization, the apparent viscosity decreased significantly, and the temperature resistance, salt resistance and shear resistance were poor.
[0072] Comparative Example 2 uses sodium 2-acrylamido-2-methylpropyl sulfonate instead of sodium fluorinated acrylate sulfonate. The obtained polyacrylamide does not contain a perfluorocarbon chain structure, and the high temperature apparent viscosity retention rate is 75.76% (15.0 / 19.8). The high salt apparent viscosity retention rate is 58.08% (11.5 / 19.8). The heat resistance, salt resistance and shear resistance are not good.
[0073] Comparative Example 3 used dodecafluoroheptyl methacrylate instead of sodium fluorinated acrylate sulfonate, and the obtained polyacrylamide did not contain sulfonic acid groups, and the high temperature apparent viscosity retention rate was 71.78% (26.2 / 36.5). The high salt apparent viscosity retention rate was 52.33% (19.1 / 36.5). The heat resistance, salt resistance and shear resistance were not good.
[0074] Comparative Example 4 uses dodecafluoroheptyl methacrylate (0.5 mmol) and sodium 2-acrylamido-2-methylpropyl sulfonate (0.5 mmol) to replace sodium fluorinated acrylate sulfonate (1 mmol). The obtained polyacrylamide does not contain sulfonic acid groups, and the high temperature apparent viscosity retention rate is 78.50% (24.1 / 30.7). The high salt apparent viscosity retention rate is 57.98% (17.8 / 30.7). It is lower than Example 1. It may be because Example 1 contains a disulfonate group and a di-perfluorocarbon chain structure. Under the condition of equal molar dosage of monomers, its sulfonate content and perfluorocarbon chain content are twice as much, so the resistance reducing agent has better temperature resistance, salt resistance and shear resistance.
[0075] The friction of deionized water and a 0.3% mass fraction of heat-resistant polyacrylamide drag reducing agent aqueous solution was tested using an annular pipe friction tester. The length of the test pipe is 6m, the inner diameter of the pipe is 10mm, and the flow rate of the solution in the pipe is controlled to be 8m / s. The pressure at the inlet and outlet of the pipe is tested and the drag reduction rate is calculated; drag reduction rate = (△F1-△F2) / △F1. △F1 is the pressure difference of deionized water at the inlet and outlet pressure of the pipe. △F2 is the pressure difference of the drag reducing agent solution at the inlet and outlet pressure of the pipe.
[0076] Table 2 Resistance reduction rate of polyacrylamide resistance reducing agent
[0077] Drag reduction rate (%) Example 1 68.7 Example 2 77.3 Example 3 71.5 Example 4 73.0 Comparative Example 1 41.6 Comparative Example 2 57.7 Comparative Example 3 54.0 Comparative Example 4 61.3
[0078] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.
Claims
1. A heat-resistant polyacrylamide drag reducing agent, characterized in that: The heat-resistant polyacrylamide drag reducing agent comprises the following raw materials: acrylamide, sodium fluorinated acrylate sulfonate, azobisisobutyramidine hydrochloride, and a surfactant in a molar ratio of (94-99):(1-6):(0.06-0.075); The fluorinated sodium acrylamide sulfonate has the following structural formula (1): Where n is 5, 6 or 7.
2. The heat-resistant polyacrylamide drag reducing agent according to claim 1, characterized in that: The surfactant is sodium dodecyl sulfate or sodium dodecylbenzene sulfonate.
3. A method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: adding acrylamide, sodium fluorinated acrylic ester sulfonate and a surfactant into deionized water, stirring and mixing, and then heating to a reaction temperature; adding azobisisobutylamidine hydrochloride in a nitrogen atmosphere; adding ethanol to precipitate after the reaction; filtering, washing with ethanol and drying to obtain a heat-resistant polyacrylamide drag reducing agent.
4. The method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 3, characterized in that: The reaction temperature is 50-65°C, and the reaction time is 4-8h.
5. The method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 3, characterized in that: The preparation method of the fluorinated sodium acrylate sulfonate is: S1. Add 1,7-bis-BOC-1,4,7-triazaheptane, 2-bromoethyl acrylate and potassium carbonate in a molar ratio of 1:(1-1.2):(1.8-2.5) to acetonitrile, heat to 40-70° C., filter after cooling, perform rotary evaporation on the filtrate, and then dissolve the product in dichloromethane and trifluoroacetic acid, stir to react for 3-4 hours, perform rotary evaporation, and perform extraction and separation to obtain intermediate 1; S2, add deionized water, sodium hydroxide and intermediate 1 to 1,4-dioxane, mix well and add 1,4-butane sultone, heat to reaction temperature, add hydrochloric acid to adjust pH of the solution to neutral after reaction, filter and rotary evaporate the filtrate, dry, wash and recrystallize to obtain intermediate 2; S3. Add intermediate 2, perfluoroacyl chloride compound and triethylamine to chloroform, react at room temperature for 24-36 hours, add deionized water, extract and separate to obtain sodium fluorinated acrylate sulfonate.
6. The method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 4, characterized in that: The molar ratio of sodium hydroxide, intermediate 1, and 1,4-butane sultone in S2 is (2-2.2):1:(2-2.2).
7. The method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 4, characterized in that: The reaction temperature in S2 is 65-75°C and the reaction time is 5-8h.
8. The method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 4, characterized in that: In S3, the molar ratio of the intermediate 2, the perfluoroacyl chloride compound and triethylamine is 1:(2.2-2.6):(2.3-2.8).
9. The method for preparing the heat-resistant polyacrylamide drag reducing agent according to claim 4, characterized in that: The structural formula of the perfluoroacyl chloride compound is Where n is 5, 6 or 7.
10. Use of the heat-resistant polyacrylamide drag reducing agent prepared by the preparation method according to any one of claims 4 to 8 in a fracturing fluid drag reducing agent.