Hydrogel micro powder as well as preparation method and application thereof

By introducing special hydrogel micropowder into the epoxy resin coating, the problems of poor mechanical properties and weak adhesion of the hydrogel are solved, the long-lasting antibacterial and antifouling function of the marine antifouling coating is achieved, and the coating's durability is ensured. Stability and antimicrobial properties.

CN118725352APending Publication Date: 2024-10-01EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410932253.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing hydrogels have poor mechanical properties and weak adhesion capabilities in the marine environment, making it difficult to meet the needs of marine antifouling coatings. In particular, their swelling properties decrease after long-term immersion, and they lack long-lasting antibacterial and antifouling functions.

Method used

Develop a hydrogel micropowder for epoxy resin coatings, which has high mechanical properties and good adhesion through specific composition ratios and preparation methods, including water-soluble polymers, guanidinium salt polymers and cross-linking agents. of hydrogel micropowder, combined with an epoxy resin coating to enhance its antibacterial and antifouling properties.

Benefits of technology

It achieves a strong combination of hydrogel micropowder and epoxy resin coating to form a durable antibacterial and antifouling coating with ideal mechanical strength and stability, which can effectively prevent biological fouling in the marine environment and extend the service life of the coating. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses hydrogel micro powder for epoxy resin as well as preparation and application of the hydrogel micro powder. The hydrogel micro powder is prepared from 70-99 parts of a water-soluble polymer, 1-30 parts of a guanidine salt polymer and 1-30 parts of a cross-linking agent (the weight part of the cross-linking agent is based on the total 100 parts of the water-soluble polymer and the guanidine salt polymer). The preparation method of the hydrogel micro powder comprises the following steps: respectively dissolving a water-soluble polymer and a guanidine salt polymer in water to prepare solutions, mixing in proportion to obtain a mixed solution, dispersing the mixed solution in an oily solvent, then cross-linking the mixed solution by using a cross-linking agent to obtain hydrogel particles, and then filtering, cleaning and drying to obtain the hydrogel micro powder. The hydrogel micro-powder is mixed into epoxy resin to form the coating, or the hydrogel micro-powder is dispersed on the surface of the epoxy resin coating and cured together with the epoxy resin coating, and the hydrogel coating which is firmly combined with the epoxy resin coating, is antibacterial, is resistant to algae adhesion and is high in mechanical strength is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical materials, and in particular to antibacterial and antifouling gel particles and a preparation method and application thereof. Background Art

[0002] The marine environment is very complex. If effective protective measures are not taken for traditional metal materials used in equipment and facilities such as ships, bridges, oil drilling platforms, and pipelines, they will usually corrode severely in a short period of time in the marine environment. Corrosion not only reduces the service life of materials and increases maintenance costs, but also endangers life and environmental safety in severe cases. In addition to seawater corrosion, marine equipment and facilities are also accompanied by serious marine biofouling. Marine biofouling refers to marine microorganisms and large organisms attached to the underwater surface of the hull or marine structure. There are many types of marine fouling organisms, among which barnacles, oysters, seaweed, etc. are the most harmful and common ones. Most of them live on the coast and in harbors.

[0003] Marine biofouling can bring serious economic, environmental and health problems to many fields related to the marine industry. For example, in the shipping industry, organisms attached to the bottom of the ship will reduce the speed of the ship. Studies have shown that the friction resistance caused by biofouling accounts for 90% of the hull resistance, resulting in an additional fuel consumption of up to 40%, causing billions of dollars in waste and hundreds of millions of tons of greenhouse gas emissions each year. At the same time, biofouling will also corrode the hull surface it contacts, shortening the service life of the ship. Fouled and attached ships will also cause cross-biological contamination, transporting marine species from a certain sea area to another new marine environment, posing a potential threat to the marine ecological environment. Applying antifouling coatings on underwater surfaces such as ships is the most convenient, effective and economical means to prevent marine organisms from attaching.

[0004] Traditional antifouling coating materials such as organotin antifouling coatings, cuprous oxide antifouling coatings, zinc oxide antifouling coatings and other bactericidal antifouling coatings contain a large amount of heavy metals, which may cause serious marine environmental crises. Since 2008, organotin antifouling coatings have been banned worldwide, and antifouling coatings using cuprous oxide as a bactericide have also been strictly restricted.

[0005] Hydrogel is a gel system formed by hydrophilic polymers and water molecules. It has a three-dimensional network structure and can swell in water but not dissolve. In the marine environment, the highly hydrophilic surface of the hydrogel will form a dynamic hydration layer after absorbing water, which has a good fouling prevention effect. Among the many new marine antifouling coating materials, hydrogel materials are considered to be the most promising candidate materials.

[0006] However, the practical application of hydrogels still faces key challenges. Hydrogels have poor mechanical properties and weak adhesion to substrates. They are easy to swell after being immersed in water, which seriously reduces their mechanical properties and adhesion. In addition to their ability to form a hydration layer and softness, they have no other anti-fouling properties. Therefore, it is of great value to research and develop new anti-sewage gels with good mechanical properties, adhesion and low swelling.

[0007] The main methods for modifying hydrogels are: (1) Nanocomposite hydrogels, which introduce nanoparticles into the polymer matrix by physical adsorption or chemical crosslinking to improve the mechanical properties of the composite hydrogel. Nanoparticles form countless crosslinking centers in the hydrogel, which can improve the strength and modulus of the material, but the agglomeration of nanoparticles is a major problem of this modification method; (2) Double network hydrogels, which use hard and brittle highly crosslinked polyelectrolytes as the first rigid network and low-crosslinked soft and tough neutral polymers as the second network. This combination can give the prepared hydrogel elasticity and ductility, and the two networks can cooperate with each other to effectively dissipate energy and improve the mechanical properties of the hydrogel. However, the preparation process of double network hydrogels is relatively complicated, and the adhesion effect is poor, which makes it difficult to meet the requirements of large-scale production and application in practical fields. Summary of the invention

[0008] The purpose of the present invention is to solve the problems of poor mechanical properties of hydrogel and weak bonding with substrates, and to provide a hydrogel micropowder and its preparation and application. The hydrogel micropowder provided by the present invention is easy to apply on the surface of epoxy resin coating, has strong bonding with epoxy resin coating, so as to exert the function of long-lasting antibacterial and antifouling of hydrogel coating.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] A hydrogel micropowder for epoxy resin coating, comprising the following components in parts by weight:

[0011] 70-99 parts of a water-soluble polymer;

[0012] 1-30 parts of a guanidine polymer;

[0013] 1-30 parts of a cross-linking agent;

[0014] The weight percentage of the crosslinking agent is based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer;

[0015] The water-soluble polymer is polyvinyl alcohol (PVA);

[0016] The guanidine polymer has a characteristic structure shown in (Formula 1):

[0017]

[0018] Wherein, Y1 and Y2 are each independently Cl - Br - 、HSO4 - 、HCO3 - 、H2PO4 - 、CH3COO - or CH3(CH2) 16 COO - , Y1 and Y2 are the same or different; m and n are natural numbers from 0 to 8, but m and n are not 0 at the same time; k is a natural number from 1 to 8;

[0019] R1 and R2 are each independently selected from one or more structural units having the structure shown in (Formula 11), the structure shown in (Formula 12), the structure shown in (Formula 13), the structure shown in (Formula 14), the structure shown in (Formula 15), the structure shown in (Formula 16) and the structure shown in (Formula 17), and R1 and R2 are the same structure or different structures;

[0020]

[0021]

[0022] R is selected from one or more structural units having the structure shown in (Formula 11), the structure shown in (Formula 12), the structure shown in (Formula 13), the structure shown in (Formula 14), the structure shown in (Formula 15), the structure shown in (Formula 16) and the structure shown in (Formula 17);

[0023] The cross-linking agent is a dialdehyde compound having a characteristic structure shown in (Formula 2), and may include one or more of glutaraldehyde, glyoxal, nonanedialdehyde, isophthalaldehyde, terephthalaldehyde, adipaldehyde, succinaldehyde, malondialdehyde, and heptanedialdehyde. Preferably, it may include one or more of glutaraldehyde, terephthalaldehyde, and adipaldehyde.

[0024] OHC-Ra-CHO (Formula 2)

[0025] Among them, Ra is selected from one or more structural units having the structure shown in (Formula 21), the structure shown in (Formula 22), the structure shown in (Formula 23), the structure shown in (Formula 24), and the structure shown in (Formula 25).

[0026]

[0027] A hydrogel micropowder for epoxy resin coating, preferably comprising the following components in parts by weight: 80-95 parts of a water-soluble polymer, 5-20 parts of a guanidine polymer, and 1-30 parts of a cross-linking agent, wherein the weight of the cross-linking agent is based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer.

[0028] A hydrogel micropowder for epoxy resin coating, preferably comprising the following components in parts by weight: 85-95 parts of a water-soluble polymer, 5-15 parts of a guanidine polymer, and 1-30 parts of a cross-linking agent, wherein the weight of the cross-linking agent is based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer.

[0029] A hydrogel micropowder for epoxy resin coating, a method for preparing a guanidine salt polymer having a structure shown in (Formula 1), comprising the following steps:

[0030] (1) selecting at least one guanidine salt having a structure represented by the general formula (3) and at least one double-terminated diamine having a structure represented by the general formula (4) to carry out a condensation polymerization reaction;

[0031]

[0032] Among them, Y n Cl - Br - 、HSO4 - 、HCO3 - 、H2PO4 - 、CH3COO - or CH3(CH2) 16 COO - , R n It is a structural unit having one or more of the structures shown in (Formula 11), (Formula 12), (Formula 13), (Formula 14), (Formula 15), (Formula 16) and (Formula 17).

[0033] (2) The material obtained in step (1) is further reacted with a double-terminal amino diamine of a structure shown in formula (4) to obtain the guanidine polymer.

[0034] The method for preparing the guanidine polymer having the structure shown in (Formula 1), wherein in step (1), the temperature of the condensation polymerization reaction is 80-180° C.;

[0035] And / or, in step (1), the condensation polymerization reaction time is 0.5-10 h, preferably 2-6 h, for example, 3.5 h, 4.5 h, 5 h or 5.5 h;

[0036] And / or, in step (1), the molar ratio of the double-terminated amino diamine of the structure represented by the general formula (4) to the guanidine salt of the structure represented by the general formula (3) is (0.8-1.2):1, preferably (0.95-1.05):1;

[0037] The method for preparing the guanidine polymer having the structure shown in (Formula 1), wherein in step (2), the reaction temperature is 80-180° C.;

[0038] And / or, in step (2), the molar amount of the diamine is 1 / 10-1 / 3 of the total molar amount of the guanidine salt of the structure represented by the general formula (3), preferably 1 / 8-1 / 4, for example, 1 / 7, 1 / 6, 1 / 5 or 1 / 4.5;

[0039] And / or, in step (2), the reaction time is 0.2-3h, preferably 0.4-2h, for example, 1.0h or 1.5h;

[0040] And / or, in step (2), the diamine is added dropwise or in batches.

[0041] The method for preparing the guanidine salt polymer of the structure shown in Formula 1, wherein in step (1), when there are at least two types of the guanidine salt of the structure shown in Formula (3) or the double-terminal amine diamine of the structure shown in Formula (4), the guanidine salt of the structure shown in Formula (3) and the double-terminal amine diamine of the structure shown in Formula (4) are arbitrarily combined and subjected to a first condensation polymerization reaction respectively, and then the materials obtained after the first condensation polymerization reaction are mixed and subjected to a second condensation polymerization reaction;

[0042] Preferably, the temperature of the first condensation polymerization reaction is 80-110°C, more preferably 85-105°C, for example, 90°C, 95°C or 100°C;

[0043] Preferably, the first condensation polymerization reaction time is 0.5-3.5h, more preferably 1-2.5h, for example, 1.5h;

[0044] Preferably, the temperature of the second condensation polymerization reaction is 140-180°C, more preferably 165-180°C, for example, 170°C or 175°C;

[0045] Preferably, the second condensation polymerization reaction time is 0.5-6.5 h, more preferably 2-5 h, for example, 3 h, 3.5 h, or 4 h.

[0046] The method for preparing the guanidine salt polymer of the structure represented by (Formula 1), wherein in step (2), the molar amount of the diamine is 1 / 10-1 / 3 of the total molar amount of the guanidine salt of the structure represented by the general formula (3), preferably 1 / 8-1 / 4, for example, 1 / 7, 1 / 6, 1 / 5 or 1 / 4.5;

[0047] and / or, in step (2), the reaction temperature is 140-180°C, more preferably 165-180°C, for example, 170°C or 175°C;

[0048] And / or, in step (2), the reaction time is 0.2-3 h, preferably 0.4-2 h, for example, 1.0 h or 1.5 h;

[0049] And / or, in step (2), the diamine is added dropwise or in batches.

[0050] The method for preparing the guanidine polymer having the structure shown in (Formula 1) comprises the following steps:

[0051] A guanidine salt having a structure shown in (Formula 31) and a guanidine salt having a structure shown in (Formula 32) are selected to respectively carry out a first condensation polymerization reaction with a double-terminal amine diamine having a structure shown in (Formula 41) and a double-terminal amine diamine having a structure shown in (Formula 42), wherein the temperature of the first condensation polymerization reaction does not exceed 80-180° C., the time of the first condensation polymerization reaction is 0.5-10 hours, and the ratio of the total molar amount of the double-terminal amine diamine to the total molar amount of the guanidine salt is (0.8-1.2):1;

[0052]

[0053] The materials after the first condensation polymerization reaction are mixed, and a second condensation polymerization reaction is carried out for 0.5-4.5 hours, and then a diamine is added, wherein the molar amount of the diamine is 1 / 10-1 / 3 of the total molar amount of the guanidine salt, and the reaction is carried out for 0.2-3 hours to obtain a guanidine salt polymer having a structure shown in (Formula 1);

[0054] Preferably, when Y1 and Y2 are the same, R1 and R2 are the same, the preparation process is carried out in the same reactor;

[0055] Preferably, when at least one of the structures of Y1 and Y2 and R1 and R2 is different, the first condensation polymerization reaction is carried out in two reactors, and the second condensation polymerization reaction is carried out in one reactor;

[0056] Preferably, the temperature of the first condensation polymerization reaction is 80-110°C, preferably 85-105°C, for example, 90°C, 95°C or 100°C;

[0057] Preferably, the first condensation polymerization reaction time is 0.5-3.5h, preferably 1-2.5h, for example, 1.5h;

[0058] Preferably, the temperature of the second condensation polymerization reaction is 140-180°C, preferably 165-180°C, for example, 170°C or 175°C;

[0059] Preferably, the second condensation polymerization reaction time is 0.5-6.5 h, preferably 2-5 h, for example, 3 h, 3.5 h, or 4 h.

[0060] A hydrogel micropowder for epoxy resin coating, the preparation process of which further comprises an auxiliary component 1, wherein the auxiliary component 1 is selected from one or more of white oil, silicone oil and vegetable oil.

[0061] Wherein, the white oil may include one or more of 5# white oil, 7# white oil, 10# white oil, 15# white oil, 26# white oil, 32# white oil, and 46# white oil.

[0062] Wherein, the silicone oil may include one or more of methyl silicone oil, ethyl silicone oil, phenyl silicone oil, methyl hydrogen silicone oil, and methylphenyl silicone oil.

[0063] Wherein, the vegetable oil may include one or more of peanut oil, soybean oil, linseed oil, castor oil and rapeseed oil.

[0064] A hydrogel micropowder for epoxy resin coating, the preparation process of which further comprises an auxiliary component 2, wherein the auxiliary component 2 is selected from any one or more of ammonium salt cationic surfactants, quaternary ammonium salt cationic surfactants, polyethylene glycol nonionic surfactants, and polyol nonionic surfactants.

[0065] Wherein, the ammonium salt surfactant and / or quaternary ammonium salt cationic surfactant may include any one or more of C8-C16 alkyl ammonium chloride, C8-C16 alkyl ammonium bromide, C8-C16 alkyl pyridine hydrochloride, C8-C16 alkyl pyridine bromate, C10-C18 alkyl trimethyl ammonium chloride, C10-C18 alkyl trimethyl ammonium bromide, C10-C18 alkyl dimethyl benzyl ammonium chloride, C8-C18 dialkyl quaternary ammonium salt, preferably include dodecyl ammonium chloride, dodecyl ammonium bromide, tetradecyl ammonium chloride, tetradecyl ammonium bromide, dodecyl pyridine hydrochloride, dodecyl pyridine bromate, dodecyl .... One or more of methylammonium chloride, dodecyltrimethylammonium bromide, tetradecyltrimethylammonium chloride, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, dodecyldimethylbenzylammonium chloride, bisoctyldimethylammonium chloride, bisoctyldimethylammonium bromide, dioctadecyldimethylammonium chloride, dioctadecyldimethylammonium bromide, didodecyldimethylammonium chloride, didodecyldimethylammonium bromide, ditetradecyldimethylammonium chloride, ditetradecyldimethylammonium bromide, dihexadecyldimethylammonium chloride, and dihexadecyldimethylammonium bromide.

[0066] Among them, the polyethylene glycol non-ionic surfactant and / or the polyol non-ionic surfactant may include C8-C18 alkyl ether polyoxyethylene, C8-C18 alkyl ester polyoxyethylene, C8-C18 alkyl amine polyoxyethylene, C8-C18 alkyl phenyl phenol polyoxyethylene, C8-C18 alkyl glyceride, C8-C18 alkyl pentaerythritol ester, Span, Tween, preferably including lauric acid glyceryl ester, palmitic acid pentaerythritol ester, nonylphenyl ether polyoxyethylene, octylphenyl ether polyoxyethylene, stearate polyoxyethylene, oleate polyoxyethylene, dodecylamine polyoxyethylene, dodecyl alcohol ether polyoxyethylene, Span 40, Span 60, Span 60, Span 80, Tween 60, Tween 65, Tween 80, Tween 85 and one or more.

[0067] A hydrogel micropowder for epoxy resin coating, the preparation process of which further includes an auxiliary component 3, and the auxiliary component 3 is water.

[0068] A hydrogel micropowder for epoxy resin coating, the preparation steps of which include:

[0069] (1) dissolving a water-soluble polymer in water to obtain an aqueous solution PS of the water-soluble polymer, wherein the concentration of the aqueous solution PS is 2-12% by mass;

[0070] (2) dissolving the guanidine polymer in water to obtain an aqueous solution GS of the guanidine polymer, wherein the concentration of the aqueous solution GS is 2-30% by mass;

[0071] (3) mixing the water-soluble polymer aqueous solution PS and the guanidine polymer aqueous solution GS, maintaining the mass ratio of the water-soluble polymer to the guanidine polymer at (70-99): (1-30), to obtain a mixed solution PS-GS;

[0072] (4) Take auxiliary component 1, add auxiliary component 2 under stirring, the mass ratio of auxiliary component 1 to auxiliary component 2 is 100:(0.5-10), and stir evenly;

[0073] (5) Adding the PS-GS mixed solution to the uniform system obtained in step (4) under stirring to form a water-in-oil dispersion, wherein the mass ratio of the PS-GS mixed solution to the dispersion is 2-40%;

[0074] (6) adding a crosslinking agent to the above-mentioned water-in-oil dispersion under stirring, wherein the weight proportion of the crosslinking agent is 1-30 parts, based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer;

[0075] (7) Under stirring conditions, hydrochloric acid was added dropwise to adjust the pH to about 3.0-4.0, and the reaction was continued for 0.5-3 hours; then sodium hydroxide solution was added dropwise to adjust the pH to greater than 9, and the reaction was continued for about 0.5-3 hours; the temperature was maintained at 20-80° C.;

[0076] (8) After the reaction is completed, the liquid is filtered out using a filter to obtain hydrogel particles, wherein the filter can be selected from a plastic filter or a metal filter;

[0077] (9) washing the hydrogel particles with an organic solvent to further remove the auxiliary component 1;

[0078] (10) washing the hydrogel particles obtained in step (9) with water to further remove the auxiliary component 2;

[0079] (11) Drying and sieving the hydrogel particles obtained in step (10) to obtain hydrogel fine powder.

[0080] Preferably, the concentration of the PS aqueous solution is 5-10%, more preferably, 8-10%.

[0081] Preferably, the concentration of the GS aqueous solution is 10-25%, more preferably, 15-20%.

[0082] Preferably, the ratio of the water-soluble polymer to the guanidine polymer is (80-95):(5-20), preferably, (85-95):

[0083] (5-15).

[0084] Preferably, the mass ratio of auxiliary component 1 to auxiliary component 2 is 100:(0.5-5).

[0085] Preferably, in the water-in-oil dispersion, the mass ratio of the PS-GS mixture to the dispersion is 10-30%, more preferably, 15-25%.

[0086] Preferably, based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer, the amount of the crosslinking agent is 3-25 parts, preferably 5-15 parts.

[0087] Preferably, the reaction temperature is 45-80°C, more preferably, 60-75°C.

[0088] Preferably, the total reaction time is 1.0-5.0 h, more preferably, 2.0-4.0 h.

[0089] The hydrogel micropowder for epoxy resin coating can be conveniently applied to the surface of epoxy resin coating to obtain a hydrogel coating with lasting antibacterial and antifouling functions. First, an epoxy resin coating is constructed on the surface of the substrate, and then the hydrogel micropowder is evenly dispersed on the surface of the epoxy resin coating so that the epoxy resin coating is completely covered by the hydrogel micropowder. After the hydrogel micropowder and the epoxy resin coating are cured together, the hydrogel micropowder and the epoxy resin coating are firmly combined together to form a hydrogel micropowder coating on the surface of the epoxy resin coating. After such a hydrogel micropowder coating is soaked in water, a layer of hydrogel coating that is firmly combined with the epoxy resin coating, has high mechanical strength, and is uniform and consistent is obtained on the surface. The formed hydrogel coating has lasting antibacterial and antifouling functions.

[0090] The hydrogel micropowder for epoxy resin coating can also be applied to epoxy resin coating by the following method. The hydrogel micropowder and epoxy resin are physically mixed in proportion to obtain a uniformly mixed epoxy resin / hydrogel micropowder composite. The mass ratio of epoxy resin to hydrogel micropowder is 100:(3-20). The uniformly mixed epoxy resin / hydrogel micropowder composite is applied to the surface of the substrate, and then cured according to the curing process of the epoxy resin, and the hydrogel micropowder and the epoxy resin coating are firmly combined together. After such an epoxy resin / hydrogel micropowder composite coating is soaked in water, a hydrogel coating that is firmly combined with the epoxy resin and has high mechanical strength is formed on the surface of the substrate. The formed hydrogel coating has the function of long-lasting antibacterial and antifouling.

[0091] In some preferred embodiments, the mass ratio of epoxy resin to hydrogel powder is 100:(10-20).

[0092] The positive beneficial effects of the present invention are:

[0093] (1) The combination of hydrogel micropowder and epoxy resin coating is very simple and easy, whether it is a construction method in which the hydrogel micropowder and epoxy resin are physically mixed in proportion and then applied on the surface of the substrate, or a construction method in which the hydrogel micropowder is dispersed on the surface of the epoxy resin coating in the form of powder spraying.

[0094] (2) The hydrogel micropowder is firmly combined with the epoxy resin coating, and the resulting hydrogel coating is strong and durable, ensuring the stability and durability of the hydrogel function.

[0095] (3) The hydrogel coating has long-lasting antibacterial and antifouling capabilities.

[0096] (4) The hydrogel coating has ideal mechanical strength, ensuring the stability and durability of the hydrogel function.

[0097] Therefore, the hydrogel powder provided by the present invention has the characteristics of simple and easy construction, and at the same time, due to its ideal mechanical strength, the function of the hydrogel is ensured to be stable and durable. In particular, the hydrogel powder can be firmly combined with the epoxy resin coating, so that the antibacterial and antifouling function of the hydrogel coating is durable, which is of great significance to the application field of marine antifouling. DETAILED DESCRIPTION

[0098] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0099] Hereinafter, exemplary embodiments of the present disclosure will be described.

[0100] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0101] The characterization of hydrogel strength, the characterization of the bonding strength between hydrogel coating and epoxy resin coating, the characterization of the antibacterial properties of hydrogel coating, the characterization of the anti-protein adhesion of hydrogel coating, and the characterization of the anti-algae adhesion of hydrogel coating are briefly described as follows.

[0102] Characterization of hydrogel strength

[0103] The hydrogel formed by the hydrogel micropowder absorbing water was used as a sample. The mechanical properties of the sheet hydrogel prepared by using a water-soluble resin matrix, guanidine polymer, crosslinker and water with exactly the same proportions were used to measure the mechanical properties of the hydrogel after the hydrogel micropowder absorbed water. The hydrogel samples were tensile tested using a universal testing machine. The tensile strength of each hydrogel sample was measured at a tensile speed of 20 mm / min at 23±2°C. The gauge length of all samples was 25 mm. Each sample was tested at least 5 times and the average value was calculated.

[0104] Characterization of the bonding strength between hydrogel coating and epoxy resin coating

[0105] The adhesion strength of the hydrogel coating and the epoxy resin coating adopts the standard "GB / T9286-2021 Scratch Test of Paint and Varnish / Paint Film". Use a grid knife to select an area on the surface of the sample to cut 10×10 small grids of 1mm×1mm, and each scratch should be as deep as possible to the substrate; use a brush to clean the residue in the test area, stick it to the small grid with 3M tape, and then use an eraser to wipe the tape hard, hold one end of the tape with both hands, make it vertical 90 degrees, and keep this angle to quickly pull off the tape. Record the number of small grids that fall off and calculate their percentage. Repeat the experiment three times at the same location to reduce the error. According to the degree of grid shedding, the adhesion can be divided into six levels from 0 to 5. Level 0 represents no shedding, and the larger the number, the more serious the shedding.

[0106] Level 0: The cutting edge is completely smooth and there is no shedding within the mesh;

[0107] Level 1: A small amount of coating falls off at the intersection of the cuts, but the affected cross-cut area is no more than 5%;

[0108] Level 2: The coating falls off at the intersection of the cuts and / or along the edges of the cuts, and the affected cross-cut area is greater than 5% but not greater than 15%;

[0109] Level 3: The coating partially or completely falls off in large pieces along the cut edge, and / or partially or completely falls off at different parts of the grid, and the affected cross-cut area is greater than 15% but not more than 35%;

[0110] Level 4: The coating falls off in large pieces along the cut edges, and / or some squares fall off partially or completely, and the affected cross-cut area is greater than 35% but not greater than 65%;

[0111] Level 5: The degree of shedding exceeds that of level 4.

[0112] Characterization of antibacterial properties of hydrogel coatings

[0113] The antibacterial properties of the hydrogel coating were tested using the film-sticking method. The steps are as follows:

[0114] (1) Cut the sample into 5 cm × 5 cm size and wash it with anhydrous ethanol for 1 min, then place it in a culture dish to dry naturally. (2) Sterilize the pipette tip, test tube, PBS buffer, and tweezers in an autoclave at 121°C for 20 min.

[0115] (3) Use PBS to prepare a concentration of 10 5CFU / mL bacterial suspension. Take 100 μL of the diluted bacterial solution and spread it evenly on the sample surface and cover it with a sterilized polyethylene film (4 cm × 4 cm), place it in a culture dish, and cover it with a lid. Place the culture dish at 37°C and relative humidity>90% for 24 hours.

[0116] (4) After the incubation period, wash the sample and the bacterial solution on the membrane three times with 10 mL of PBS buffer solution.

[0117] Collect the washed bacterial solution and dilute it in 10-fold gradients. Take 100 μL of the bacterial solution with different dilutions with a pipette, drop it on the sterile agar culture dish and spread it evenly. Put the agar culture dish with bacteria inverted and put it in a 37℃ constant temperature incubator for 24 hours, observe the growth of bacteria and count the number of colonies.

[0118] The inhibition rate was calculated according to formula (51).

[0119]

[0120] Among them, A represents the colony count of the blank control group, and B represents the colony count of the hydrogel coating sample.

[0121] The antifouling properties of the hydrogel coating were characterized by the anti-protein adhesion properties of the hydrogel coating and the anti-algae adhesion properties of the hydrogel.

[0122] Characterization of hydrogel coatings against protein adhesion

[0123] The ultraviolet absorption method was used to analyze the amount of protein adsorbed by the hydrogel coating and to test the anti-protein adsorption performance of the hydrogel coating.

[0124] Weigh 1.134g of disodium hydrogen phosphate and 0.544g of potassium dihydrogen phosphate respectively, add 400mL of deionized water to dissolve and prepare PBS standard buffer solution. Add bovine serum albumin (BSA) to the PBS buffer solution to prepare BSA solutions of different concentrations (0.1mg / mL, 0.2mg / mL, 0.3mg / mL, 0.4mg / mL, 0.5mg / mL). Measure the ultraviolet absorbance of the above BSA solution with a UV-visible spectrophotometer, and then establish a standard curve of absorbance and concentration at the characteristic wavelength (278nm) of BSA.

[0125] Cut the hydrogel coating sample into 20×20 mm 2Three pieces of each size were washed with anhydrous ethanol and PBS buffer solution for 30 minutes respectively, and then placed in 10mL 0.5mg / mL BSA solution, kept at 25℃ for 24h, and the samples were taken out after the adsorption reached equilibrium. The absorbance of the remaining BSA solution at 278nm was tested. According to the above standard curve, the concentration of the remaining BSA in the solution can be obtained, and then the amount of BSA adsorbed on the sample can be calculated.

[0126] After the hydrogel coating was placed in water for 6 months, it was taken out and simply rinsed with clean water, and then the anti-protein adhesion performance of the hydrogel coating was tested again using the above test method.

[0127] Characterization of hydrogel coatings against algae adhesion

[0128] In order to test the anti-algae performance of the hydrogel coating, a common algae, Chlorella vulgaris, was selected to conduct an adhesion experiment on the coating sample. First, Chlorella vulgaris was transferred to the culture medium and cultured to an appropriate concentration. The illumination conditions during the culture were controlled at 5000 lux, and the light-dark cycle ratio was 14:10. The hydrogel coating sample was cut into 20×20 mm 2 The slices were placed into 10 ml of Chlorella suspension. The initial Chlorella suspension density was measured by microscope to be 5×10 6 After the coated samples were cultured in the container for 14 days, they were washed with homemade seawater to remove loosely attached algae. The samples were then placed under a microscope for observation and the number of Chlorella attached was counted.

[0129] After the hydrogel coating was placed in water for 6 months, it was taken out and simply rinsed with clean water, and the anti-algae adhesion performance of the hydrogel coating was tested again using the above test method.

[0130] Example 1

[0131] 5g of powdered PVA1799 was added to 45g of water under stirring, and then heated to 90°C while stirring, and continued stirring until PVA1799 was completely dissolved in the water to obtain a 10% PVA1799 aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer 1 (where R1 and R2 in the structure of (Formula 1) are hexamethylene and pentamethylene, respectively, R is hexamethylene, and Y1 and Y2 are both Cl - ), add it to 4g water under stirring, and continue stirring until the guanidine polymer 1 is completely dissolved in the water to obtain a 20% guanidine polymer aqueous solution GS. Mix 50g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 1 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 5:1, to obtain a mixed solution PS-GS, 55g.

[0132] Take 300g of No. 7 white oil, then add 2.4g of Span 80 and 1.2g of Tween 80, a nonionic surfactant, under stirring, and stir evenly. Then, under stirring, slowly add 55g of PS-GS mixed solution to the mixed system of white oil and nonionic surfactant to form an oil-in-water dispersion of white oil-coated PS-GS mixed solution. Then, add 1g of glutaraldehyde to the above-mentioned oil-in-water dispersion under stirring. Under stirring, adjust the pH to 3.5 with hydrochloric acid, heat to 60°C, and react for 1.5h. Then, adjust the pH to 9.5 with sodium hydroxide solution, and continue to react for 1.5h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. The hydrogel particles are fully washed with xylene to remove the white oil. Then wash with water to remove the surfactant. The cleaned hydrogel particles are dried and sieved to obtain hydrogel micropowder 1.

[0133] Example 2

[0134] 5g of powdered PVA1799 was added to 45g of water under stirring, and then heated to 90°C while stirring, and continued stirring until PVA was completely dissolved in the water to obtain a 10% PVA aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer 2 (wherein R1 and R2 in the structure of (Formula 1) are both hexamethylene, R is hexamethylene, and Y1 and Y2 are both Cl - ), add it to 4g water under stirring, and continue stirring until the guanidine polymer 2 is completely dissolved in the water to obtain a 20% guanidine polymer aqueous solution GS. Mix 50g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 2 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 5:1, to obtain a mixed solution PS-GS, 55g.

[0135] Take 300g of No. 7 white oil, then add 2.4g of Span 80 and 1.2g of Tween 80, a nonionic surfactant, under stirring, and stir evenly. Then, under stirring, slowly add 55g of PS-GS mixed solution to the mixed system of white oil and nonionic surfactant to form an oil-in-water dispersion of white oil-coated PS-GS mixed solution. Then, add 1.2g of isophthalaldehyde to the above oil-in-water dispersion under stirring. Under stirring, adjust the pH to 3.5 with hydrochloric acid, heat to 60°C, and react for 1.5h. Then, adjust the pH to 9.5 with sodium hydroxide solution, and continue to react for 1.5h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. The hydrogel particles are fully washed with n-hexane to remove the white oil. Then wash with water to remove the surfactant. The cleaned hydrogel particles are dried and sieved to obtain hydrogel micropowder 2.

[0136] Example 3

[0137] 10g of powdered PVA1788 was added to 90g of water under stirring, and then heated to 90°C while stirring, and continued stirring until PVA was completely dissolved in the water to obtain a 10% PVA aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer 3 (wherein R1 and R2 in the structure of (Formula 1) are hexamethylene and benzene ring, respectively, R is hexamethylene, and Y1 and Y2 are both Cl - ), add it to 4g water under stirring, and continue stirring until the guanidine polymer 3 is completely dissolved in the water to obtain a 20% guanidine polymer aqueous solution GS. Mix 100g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 3 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 10:1, to obtain a mixed solution PS-GS, 105g.

[0138] Take 500g of No. 7 white oil, then add 4.0g of Span 80 and 2.0g of Tween 80, a nonionic surfactant, under stirring, and stir evenly. Then, under stirring, slowly add 105g of PS-GS mixture to the mixed system of white oil and surfactant to form an oil-in-water dispersion of white oil-coated PS-GS mixture. Then, add 2g of adipaldehyde to the above oil-in-water dispersion under stirring. Under stirring, adjust the pH to 4.0 with hydrochloric acid, heat to 60°C, and react for 2.0h. Then, adjust the pH to 9.5 with sodium hydroxide solution, and continue to react for 1.0h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. The hydrogel particles are fully washed with n-hexane to remove the white oil. Then wash with water to remove the surfactant. The cleaned hydrogel particles are dried and sieved to obtain hydrogel micropowder 3.

[0139] Example 4

[0140] 5g of powdered PVA2499 was added to 45g of water under stirring, and then heated to 95°C while stirring, and continued stirring until the starch was completely dissolved in the water to obtain a 10% PVA aqueous solution PS, which was cooled to room temperature for use. 1.5g of guanidine polymer 4 (wherein R1 and R2 in the structure of (Formula 1) are hexamethylene and pentamethylene, respectively, R is a benzene ring, and Y1 and Y2 are both Cl - ), add it to 3.5g water under stirring, and continue stirring until the guanidine polymer 4 is completely dissolved in the water to obtain a 30% guanidine polymer aqueous solution GS. Mix 50g of 10% PVA aqueous solution PS and 5g of 30% guanidine polymer 4 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 5:1.5, to obtain a mixed solution PS-GS, 55g.

[0141] Take 300g of No. 15 white oil, then add 3g of nonionic surfactant Tween 80 under stirring conditions and stir evenly. Then, under stirring conditions, slowly add the PS-GS mixture to the mixed system of white oil and Tween 80 to form an oil-in-water dispersion of the white oil-coated PS-GS mixture. Then, add 1g of glutaraldehyde to the above-mentioned oil-in-water dispersion under stirring conditions. Under stirring conditions, adjust the pH to 3.5 with hydrochloric acid, heat to 65°C, and react for 1.5h. Then, adjust the pH to 9.5 with sodium hydroxide solution and continue to react for 1.0h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. The hydrogel particles are fully washed with cyclohexane to remove the white oil. Then wash with water to remove the surfactant. The cleaned hydrogel particles are dried and sieved to obtain hydrogel micropowder 4.

[0142] Example 5

[0143] 10g of powdered PVA1799 was added to 90g of water under stirring, and then heated to 90°C while stirring, and continued stirring until PVA was completely dissolved in the water to obtain a 10% PVA aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer 5 (wherein R1 and R2 in the structure of (Formula 1) are hexamethylene and pentamethylene, respectively, R is hexamethylene, and Y1 and Y2 are both H2PO4 - ), add it to 4g water under stirring, and continue stirring until the guanidine polymer 5 is completely dissolved in the water to obtain a 20% aqueous solution GS of the guanidine polymer 5. Mix 100g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 5 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 10:1, to obtain a mixed solution PS-GS, 105g.

[0144] Take 500g of No. 7 white oil, then add 3g of non-ionic surfactant Tween 80 under stirring conditions and stir evenly. Then, under stirring conditions, slowly add the PS-GS mixture to the mixed system of white oil and Tween 80 to form an oil-in-water dispersion of the white oil-coated PS-GS mixture. Then, add 1.5g of glutaraldehyde to the above-mentioned oil-in-water dispersion under stirring conditions. Under stirring conditions, heat to 60°C and react for 4h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. Wash the hydrogel particles thoroughly with xylene to remove the white oil. Then wash with water to remove the surfactant Tween. Dry the cleaned hydrogel particles and sieve them to obtain hydrogel micropowder 5.

[0145] Example 6

[0146] 10g of powdered PVA1799 was added to 90g of water under stirring, and then heated to 90°C while stirring, and continued stirring until PVA was completely dissolved in the water to obtain a 10% PVA aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer 6 (where R1 and R2 in the structure of (Formula 1) are hexamethylene and pentamethylene, respectively, R is hexamethylene, and Y1 and Y2 are both HSO4 - ), add it to 4g water under stirring, and continue stirring until the guanidine polymer 6 is completely dissolved in the water to obtain a 20% aqueous solution GS of guanidine polymer 6. Mix 100g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 6 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 10:1, to obtain a mixed solution PS-GS, 105g.

[0147] Take 500g of No. 7 white oil, then add 3g of non-ionic surfactant Tween 80 under stirring conditions and stir evenly. Then, under stirring conditions, slowly add the PS-GS mixture to the mixed system of white oil and Tween 80 to form an oil-in-water dispersion of the white oil-coated PS-GS mixture. Then, add 1.5g of glutaraldehyde to the above-mentioned oil-in-water dispersion under stirring conditions. Under stirring conditions, heat to 60°C and react for 4h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. Wash the hydrogel particles thoroughly with xylene to remove the white oil. Then wash with water to remove the surfactant Tween. Dry the cleaned hydrogel particles and sieve them to obtain hydrogel micropowder 6.

[0148] Comparative Example 1

[0149] 5g of powdered PVA1799 was added to 45g of water under stirring, and then heated to 90°C while stirring, and continued stirring until PVA1799 was completely dissolved in the water to obtain a 10% PVA1799 aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer 1 (where R1 and R2 in the structure of (Formula 1) are hexamethylene and pentamethylene, respectively, R is hexamethylene, and Y1 and Y2 are both Cl - ), add it to 4g water under stirring, and continue stirring until the guanidine polymer 1 is completely dissolved in the water to obtain a 20% guanidine polymer aqueous solution GS. Mix 50g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 1 aqueous solution GS, at which the ratio of PVA to guanidine polymer is 5:1, to obtain a mixed solution PS-GS, 55g.

[0150] Take 300g of No. 7 white oil, then add 2.4g of Span 80 and 1.2g of Tween 80, a nonionic surfactant, under stirring, and stir evenly. Then, under stirring, slowly add 55g of PS-GS mixed solution to the mixed system of white oil and nonionic surfactant to form an oil-in-water dispersion of white oil-coated PS-GS mixed solution. Under stirring, adjust the pH to 3.5 with hydrochloric acid, heat to 60°C, and react for 1.5h. Then, adjust the pH to 9.5 with sodium hydroxide solution, and continue to react for 1.5h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh, and no hydrogel particles are obtained.

[0151] Comparative Example 2

[0152] 10 g of powdered PVA1799 was added to 90 g of water under stirring, and then heated to 90°C while stirring. Stirring was continued until PVA was completely dissolved in the water to obtain a 10% PVA aqueous solution PS, which was then cooled to room temperature for use.

[0153] Take 500g of No. 7 white oil, then add 3g of non-ionic surfactant Tween 80 under stirring conditions and stir evenly. Then, under stirring conditions, slowly add 10% PVA aqueous solution to the mixed system of white oil and Tween 80 to form an oil-in-water type dispersion of white oil-coated PS mixed liquid. Then, add 1.5g of glutaraldehyde to the above oil-in-water type dispersion under stirring conditions. Under stirring conditions, heat to 60°C and react for 4h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. Wash the hydrogel particles thoroughly with xylene to remove the white oil. Then wash with water to remove the surfactant Tween. Dry the cleaned hydrogel particles and sieve them to obtain hydrogel micropowder-to-2.

[0154] Comparative Example 3

[0155] 5g of powdered PVA1799 was added to 45g of water under stirring conditions, and then heated to 90°C while stirring, and continued to stir until PVA1799 was completely dissolved in water to obtain a 10% PVA1799 aqueous solution PS, which was cooled to room temperature for use. 1g of guanidine polymer X (specific structure see formula 61) was added to 4g of water under stirring conditions, and continued to stir until guanidine polymer 1 was completely dissolved in water to obtain a 20% guanidine polymer aqueous solution GS. 50g of 10% PVA aqueous solution PS and 5g of 20% guanidine polymer 1 aqueous solution GS were mixed, and the ratio of PVA to guanidine polymer was 5:1 at this time, and a mixed solution PS-GS, 55g, was obtained.

[0156] Take 300g of No. 7 white oil, then add 2.4g of Span 80 and 1.2g of Tween 80, a nonionic surfactant, under stirring, and stir evenly. Then, under stirring, slowly add 55g of PS-GS mixed solution to the mixed system of white oil and nonionic surfactant to form an oil-in-water dispersion of white oil-coated PS-GS mixed solution. Then, add 1g of glutaraldehyde to the above oil-in-water dispersion under stirring. Under stirring, adjust the pH to 3.5 with hydrochloric acid, heat to 60°C, and react for 1.5h. Then, adjust the pH to 9.5 with sodium hydroxide solution, and continue to react for 1.5h. After the reaction is completed, filter and remove the liquid with a 200-mesh metal mesh to obtain hydrogel particles. The hydrogel particles are fully washed with xylene to remove the white oil. Then wash with water to remove the surfactant. The cleaned hydrogel particles are dried and sieved to obtain hydrogel micropowder-to-3.

[0157]

[0158] Wherein, m is a natural number from 1 to 8;

[0159] The data of Examples 1-6 and Comparative Examples 1-3 are listed in Table 1.

[0160] Table 1

[0161]

[0162] Micro powder application example 1

[0163] First, an epoxy resin coating is applied to the surface of the steel material, and then the hydrogel powder 1 of Example 1 is evenly dispersed on the surface of the epoxy resin coating. The hydrogel powder participates in the curing of the epoxy resin coating and is firmly combined with the epoxy resin coating, thereby forming a hydrogel powder coating on the surface of the epoxy resin coating. After such a hydrogel powder coating is soaked in water, a hydrogel coating that is firmly combined with the epoxy coating, has high mechanical strength, and is durable in antibacterial and antifouling is obtained on the surface. The properties of the hydrogel coating are shown in Table 2.

[0164] Micro powder application example 2

[0165] First, an epoxy resin coating is applied to the surface of the steel material, and then the hydrogel powder 2 of Example 2 is evenly dispersed on the surface of the epoxy resin coating. The hydrogel powder participates in the curing of the epoxy resin coating and is firmly combined with the epoxy resin coating, thereby forming a hydrogel powder coating on the surface of the epoxy resin coating. After such a hydrogel powder coating is soaked in water, a hydrogel coating that is firmly combined with the epoxy coating, has high mechanical strength, and is durable in antibacterial and antifouling is obtained on the surface. The properties of the hydrogel coating are shown in Table 2.

[0166] Micro powder application example 3

[0167] First, the epoxy resin coating is applied to the surface of the steel material, and then the hydrogel powder 3 of Example 3 is evenly dispersed on the surface of the epoxy resin coating. The hydrogel powder participates in the curing of the epoxy resin coating and is firmly combined with the epoxy resin coating, thereby forming a hydrogel powder coating on the surface of the epoxy resin coating. After such a hydrogel powder coating is soaked in water, a hydrogel coating that is firmly combined with the epoxy coating, has high mechanical strength, and is durable in antibacterial and antifouling is obtained on the surface. The properties of the hydrogel coating are shown in Table 2.

[0168] Application Example 1

[0169] First, the epoxy resin coating is applied to the surface of the steel material, and then the hydrogel powder-to-2 of the comparative example 2 is evenly dispersed on the surface of the epoxy resin coating. The hydrogel powder and the epoxy resin coating are cured together, thereby forming a hydrogel powder coating on the surface of the epoxy resin coating. After such a hydrogel powder coating is soaked in water, a hydrogel coating is obtained on the surface. The properties of the hydrogel coating are shown in Table 2.

[0170] Application Example 2

[0171] First, the epoxy resin coating is applied to the surface of the steel material, and then the hydrogel powder of the comparative example 3 is evenly dispersed on the surface of the epoxy resin coating. The hydrogel powder participates in the curing of the epoxy resin coating and is firmly combined with the epoxy resin coating, thereby forming a hydrogel powder coating on the surface of the epoxy resin coating. After such a hydrogel powder coating is soaked in water, a hydrogel coating is obtained on the surface. The properties of the hydrogel coating are shown in Table 2.

[0172] The results in Table 2 show that the epoxy resin coating without hydrogel micropowder has relatively poor anti-protein adhesion and anti-algae adhesion properties. In Application Example 1, Application Example 2 and Application Example 3, the hydrogel micropowder has a good bonding strength with the epoxy resin coating, and the formed surface has good antibacterial, anti-protein adhesion and anti-algae adhesion properties, and after staying in water for a long time, it still maintains good antibacterial, anti-protein adhesion and anti-algae adhesion properties. In Application Control Example 1, the hydrogel micropowder without guanidine polymer-powder 2 has a low bonding strength with the epoxy resin coating, and the anti-protein adhesion and anti-algae adhesion properties are also reduced. In Application Control Example 2, the hydrogel micropowder coating has good antibacterial, anti-protein adhesion and anti-algae adhesion properties, but the mechanical strength of the hydrogel coating is worse than that of the hydrogel coating in Application Example 1, Application Example 2 and Application Example 3. It can be seen that the new hydrogel powder disclosed by the present invention, when applied to the surface of epoxy resin coating, not only has a good bonding strength with the epoxy resin coating, but also has long-term antibacterial, anti-protein adhesion and anti-algae adhesion properties.

[0173] Table 2

[0174]

[0175] Finally, it should be noted that in the present invention, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements that are inherent to such process, method, article or apparatus.

[0176] Although the present disclosure has been disclosed above through the description of the specific embodiments of the present disclosure, it should be understood that those skilled in the art can design various modifications, improvements or equivalents to the present disclosure within the spirit and scope of the attached scheme. These modifications, improvements or equivalents should also be considered to be included in the scope of protection claimed by the present disclosure.

Claims

1. A hydrogel micropowder for epoxy resin coating, It is characterized in that The invention comprises the following components in parts by weight: 70-99 parts of a water-soluble polymer, 1-30 parts of a guanidine polymer, and 1-30 parts of a cross-linking agent, wherein the weight of the cross-linking agent is based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer; The water-soluble polymer is polyvinyl alcohol (PVA); The guanidine polymer has the following characteristic structure: Among them, Y 1 and Y 2 Each independently is Cl - Br - , HSO 4 - , HCO 3 - , H 2 PO 4 - , CH 3 COO - or CH 3 (CH 2 ) 16 COO - , Y 1 and Y 2 The two are the same or different; m and n are natural numbers from 0 to 8, but m and n are not 0 at the same time; k is a natural number from 1 to 8; R 1 and R 2 Each independently selected from one or more structural units having the structure shown in (Formula 11), the structure shown in (Formula 12), the structure shown in (Formula 13), the structure shown in (Formula 14), the structure shown in (Formula 15), the structure shown in (Formula 16) and the structure shown in (Formula 17), R 1 and R 2 The two are of the same structure or of different structures; R is selected from one or more structural units having the structure shown in (Formula 11), the structure shown in (Formula 12), the structure shown in (Formula 13), the structure shown in (Formula 14), the structure shown in (Formula 15), the structure shown in (Formula 16) and the structure shown in (Formula 17); The crosslinking agent is a dialdehyde compound selected from one or more of glutaraldehyde, glyoxal, nonanedialdehyde, isophthalaldehyde, terephthalaldehyde, adipaldehyde, succinaldehyde, malondialdehyde, and heptanedialdehyde, preferably, selected from one or more of glutaraldehyde, terephthalaldehyde, and adipaldehyde.

2. A hydrogel micropowder for epoxy resin coating as claimed in claim 1, It is characterized in that The invention comprises the following components in parts by weight: 80-95 parts of a water-soluble polymer, 5-20 parts of a guanidine polymer, and 1-30 parts of a cross-linking agent, wherein the weight of the cross-linking agent is based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer.

3. A hydrogel micropowder for epoxy resin coating according to any one of claims 1 to 2, It is characterized in that The preparation method of the guanidine polymer comprises the following steps: (1) selecting at least one guanidine salt having a structure represented by the general formula (3) and at least one double-terminal amino diamine having a structure represented by the general formula (4) to carry out a condensation polymerization reaction; (2) The material obtained in step (1) is further reacted with a double-terminal amino diamine having a structure shown in formula (4) to obtain the guanidine polymer.

4. The method for preparing the guanidine polymer according to claim 3, It is characterized in that In step (1), the temperature of the condensation polymerization reaction is 80-180°C; And / or, in step (1), the condensation polymerization reaction time is 0.5-10 h, preferably 2-6 h, for example, 3.5 h, 4.5 h, 5 h or 5.5 h; And / or, in step (1), the molar ratio of the double-terminal amino diamine of the structure represented by the general formula (4) to the guanidine salt of the structure represented by the general formula (3) is (0.8-1.2):1, preferably (0.95-1.05):1; And / or, in step (2), the molar amount of the diamine is 1 / 10-1 / 3 of the total molar amount of the guanidine salt of the structure represented by the general formula (3), preferably 1 / 8-1 / 4, for example, 1 / 7, 1 / 6, 1 / 5 or 1 / 4.5; And / or, in step (2), the reaction time is 0.2-3h, preferably 0.4-2h, for example, 1.0h or 1.5h; And / or, in step (2), the diamine is added dropwise or in batches.

5. The method for preparing the guanidine polymer according to claim 3 or 4, It is characterized in that In step (1), when there are at least two types of the guanidine salt of the structure represented by the general formula (3) or the double-terminal amine diamine of the structure represented by the general formula (4), the guanidine salt of the structure represented by the general formula (3) and the double-terminal amine diamine of the structure represented by the general formula (4) are arbitrarily combined to perform a first condensation polymerization reaction respectively, and then the materials obtained after the first condensation polymerization reaction are mixed and a second condensation polymerization reaction is performed; Preferably, the temperature of the first condensation polymerization reaction is 80-110°C, more preferably 85-105°C, for example, 90°C, 95°C or 100°C; Preferably, the first condensation polymerization reaction time is 0.5-3.5h, more preferably 1-2.5h, for example, 1.5h; Preferably, the temperature of the second condensation polymerization reaction is 140-180°C, more preferably 165-180°C, for example, 170°C or 175°C; Preferably, the second condensation polymerization reaction time is 0.5-6.5 h, more preferably 2-5 h, for example, 3 h, 3.5 h or 4 h.

6. The method for preparing the guanidine polymer according to claim 3 or 4, It is characterized in that The preparation method of the guanidine polymer comprises the following steps: A guanidine salt of structure shown in (Formula 31) and a guanidine salt of structure shown in (Formula 32) are selected to respectively carry out a first condensation polymerization reaction with a double-terminal amine diamine of structure shown in (Formula 41) and a double-terminal amine diamine of structure shown in (Formula 42), wherein the temperature of the first condensation polymerization reaction is 80-180° C., the time of the first condensation polymerization reaction is 0.5-10 hours, and the ratio of the total molar amount of the double-terminal amine diamine to the total molar amount of the guanidine salt is (0.8-1.2):1; The materials after the first condensation polymerization reaction are mixed, and a second condensation polymerization reaction is carried out for 0.5-4.5 hours, and then a diamine is added, wherein the molar amount of the diamine is 1 / 10-1 / 3 of the total molar amount of the guanidine salt, and the reaction is carried out for 0.2-3 hours to obtain the guanidine salt polymer; Preferably, when Y 1 and Y 2 Same, R 1 and R 2 The same, the preparation process is carried out in the same reactor; Preferably, when Y 1 and Y 2 Between 1 and R 2 If at least one group of structures is different, the first condensation polymerization reaction is carried out in two reactors, and the second condensation polymerization reaction is carried out in one reactor; Preferably, the temperature of the first condensation polymerization reaction is 80-110°C, preferably 85-105°C, for example, 90°C, 95°C or 100°C; Preferably, the first condensation polymerization reaction time is 0.5-3.5h, preferably 1-2.5h, for example, 1.5h; Preferably, the temperature of the second condensation polymerization reaction is 140-180°C, preferably 165-180°C, for example, 170°C or 175°C; Preferably, the second condensation polymerization reaction time is 0.5-6.5 h, preferably 2-5 h, for example, 3 h, 3.5 h or 4 h.

7. A hydrogel micropowder for epoxy resin coating according to any one of claims 1 to 2, It is characterized in that It also includes auxiliary component 1, which is selected from one or more of white oil, silicone oil, and vegetable oil; it also includes auxiliary component 2, which is selected from one or more of cationic surfactants and non-ionic surfactants; it also includes auxiliary component 3, which is water.

8. A hydrogel micropowder for epoxy resin coating as claimed in claims 1 to 6, It is characterized in that The preparation steps include: (1) dissolving a water-soluble polymer in water to obtain an aqueous solution PS of the water-soluble polymer, wherein the concentration of the aqueous solution PS is 2-12% by mass; (2) dissolving the guanidine polymer in water to obtain an aqueous solution GS of the guanidine polymer, wherein the concentration of the aqueous solution GS is 2-30% by mass; (3) mixing a water-soluble polymer aqueous solution PS and a guanidine polymer aqueous solution GS, maintaining a ratio of the water-soluble polymer to the guanidine polymer of (70-99):(1-30), to obtain a mixed solution PS-GS; (4) Take auxiliary component 1, add auxiliary component 2 under stirring conditions, and stir evenly; (5) Adding the PS-GS mixed solution to the uniform system obtained in step (4) under stirring to form a water-in-oil dispersion, wherein the mass ratio of the PS-GS mixed solution to the dispersion is 2-40%; (6) adding a crosslinking agent to the above-mentioned water-in-oil dispersion under stirring, wherein the weight proportion of the crosslinking agent is 1-30 parts, based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer; (7) Under stirring conditions, hydrochloric acid was added dropwise to adjust the pH to about 3.0-4.0, and the reaction was continued for 0.5-3 hours; then sodium hydroxide solution was added dropwise to adjust the pH to greater than 9, and the reaction was continued for about 0.5-3 hours; the temperature was maintained at 20-80° C.; (8) After the reaction is completed, the liquid is filtered out using a filter to obtain hydrogel particles; (9) washing the hydrogel particles with an organic solvent to further remove the auxiliary component 1; (10) washing the hydrogel particles obtained in step (9) with water to further remove the auxiliary component 2; (11) Drying and sieving the hydrogel particles obtained in step (10) to obtain hydrogel fine powder. Preferably, the concentration of the PS aqueous solution is 5-10%, more preferably, 8-10%; Preferably, the concentration of the GS aqueous solution is 10-25%, more preferably, 15-20%; Preferably, the ratio of the water-soluble polymer to the guanidine polymer is (80-95):(5-20), preferably, (85-95): (5-15); Preferably, in the water-in-oil dispersion, the mass ratio of the PS-GS mixture to the dispersion is 10-30%, preferably 15-25%; Preferably, based on 100 parts of the total amount of the water-soluble polymer and the guanidine polymer, the amount of the crosslinking agent is 3-25 parts, preferably, 5-15 parts; Preferably, the reaction temperature is 45-80°C, more preferably, 60-75°C; Preferably, the reaction time is 1.0-5.0 h, more preferably, 2.0-4.0 h.

9. A hydrogel micropowder for epoxy resin coating according to claims 1-2 and / or claim 8, It is characterized in that The method can be applied to the surface of epoxy resin coating: the hydrogel powder is evenly dispersed and completely covered on the surface of epoxy resin coating, and is firmly combined with the epoxy resin coating to form a hydrogel powder coating; or the epoxy resin and the hydrogel powder are evenly mixed in a mass ratio of 100:(3-20), and then a coating is prepared using the evenly mixed mixture. After the mixture coating is cured, the hydrogel powder and the epoxy resin are firmly combined to form a hydrogel powder coating.

10. The hydrogel micropowder coating on the surface of the epoxy resin coating as claimed in claim 9, It is characterized in that The obtained hydrogel micropowder coating has durable antibacterial and antifouling functions.