Preparation method and application of modified chitosan microsphere double-container corrosion inhibitor

By introducing cyclodextrin into the chitosan molecular chain, a modified chitosan microsphere dual-container corrosion inhibitor is prepared, which solves the problem of carbon dioxide corrosion in oil and gas fields, achieves effective protection of CO2, and significantly reduces the degree of corrosion. Demonstrates excellent anti-corrosion properties.

CN118725355APending Publication Date: 2024-10-01CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410905952.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In oil and gas fields, carbon dioxide corrosion problems occur frequently, leading to corrosion of pipelines and equipment. In severe cases, it may cause perforations and safety accidents. The existing micro/nano container designs have a single function and no corrosion inhibition effect, and lack effective resistance to CO2 corrosion.

Method used

By introducing a cyclodextrin intermediate into the natural chitosan molecular chain, a modified chitosan microsphere dual-container corrosion inhibitor is prepared, the corrosion inhibitor is loaded and transported to the corrosion area through targeted transportation, forming a dense film of synergistic corrosion inhibition. , reduce corrosion.

Benefits of technology

Effectively inhibit CO2 corrosion, significantly increase the load type and quantity of corrosion inhibitors, form a protective film, significantly reduce the degree of corrosion on the steel surface, and demonstrate excellent anti-corrosion performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725355A_ABST
    Figure CN118725355A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a modified chitosan double-container microsphere corrosion inhibitor, which comprises the following steps: dissolving benzotriazole in an acetone solution, stirring until the benzotriazole is dissolved, adding the benzotriazole into a flask of a water solution containing beta-cyclodextrin, and stirring at a constant temperature; after the reaction is finished, carrying out suction filtration, washing with deionized water, and drying to obtain an intermediate product; adding the intermediate product into a flask containing a sodium hydroxide solution, and stirring until the intermediate product is dissolved; dropwise adding a paratoluensulfonyl chloride solution dissolved in acetonitrile into the flask, and stirring at a constant temperature; after the reaction is finished, carrying out suction filtration on the solution, washing with deionized water, and drying to obtain an intermediate product; adding chitosan and 1-allylimidazole into a flask containing an acetic acid solution, and stirring until the chitosan and the 1-allylimidazole are dissolved; dissolving the intermediate product in a DMF (Dimethyl Formamide) solution, stirring until the intermediate product is dissolved, dropwise adding into a flask, and stirring at constant temperature; after the reaction is finished, dropwise adding the solution into a flask containing liquid paraffin and Span80, and mechanically stirring at constant temperature; dropwise adding a glutaraldehyde solution into the flask, and mechanically stirring at constant temperature; and after the reaction is finished, centrifuging the obtained emulsion, washing the product with petroleum ether and isopropanol in sequence, and collecting and drying to obtain the modified chitosan double-container microsphere corrosion inhibitor. The environment-friendly polymer chitosan is selected as the raw material, the prepared corrosion inhibitor has excellent corrosion resistance in the CO2 environment, long-term stable operation of pipes and equipment can be guaranteed, and the corrosion inhibitor has wide development prospects and application potential in the field of corrosion prevention of oil and gas fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oilfield chemical corrosion inhibitor anticorrosion, and in particular to a preparation method and application of a modified chitosan microsphere double-container corrosion inhibitor. Background Art

[0002] Carbon dioxide (CO2) corrosion frequently occurs in oil and gas field exploitation, especially in the development of deep CO2 gas reservoirs and the application of CO2 injection enhanced production technology in oil fields. This corrosion phenomenon not only leads to comprehensive corrosion and local corrosion of pipelines and equipment, but also causes perforation in severe cases, resulting in huge economic losses and even serious safety accidents. In recent years, micro / nano containers have developed into a highly innovative corrosion inhibitor design method. However, many containers have problems such as single function and no corrosion inhibition effect. Therefore, the development and synthesis of a new pH-responsive dual-container loading system with excellent anti-CO2 corrosion performance is extremely important for the protection of carbon dioxide corrosion in oil and gas fields. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a modified chitosan double-container microsphere corrosion inhibitor. The present invention modifies the natural polysaccharide chitosan molecule, and introduces a cyclodextrin intermediate on part of the amino group of the chitosan molecular chain to prepare a double-container system, so that the corrosion inhibitor can be loaded in the cyclodextrin cavity and inside the microsphere, respectively, thereby increasing the type and quantity of the loaded corrosion inhibitor. The container is targeted and transported to the corrosion area, and the chitosan molecules and the corrosion inhibitor released by the container play a synergistic corrosion inhibition role, and a denser corrosion inhibitor film is formed on the steel surface, effectively alleviating corrosion. It is applied to oil and gas field corrosion protection, which can effectively inhibit the CO2 corrosion problem faced by oil and gas fields, and has broad industrial application prospects. The present invention also provides its preparation method and application.

[0004] To achieve the above objectives, the present invention adopts the following technical solutions.

[0005] A method for preparing a modified chitosan microsphere double-container corrosion inhibitor comprises the following steps in sequence:

[0006] (1) Dissolve benzotriazole (BTA) in acetone solution, mix and stir until BTA is completely dissolved. Then add the dissolved solution into a flask containing an aqueous solution of β-cyclodextrin (β-CD), and stir at a constant temperature for 2 hours;

[0007] (2) filtering the solution and washing it with deionized water, collecting and drying it to obtain an intermediate product;

[0008] (3) Add the intermediate product obtained in step (2) into a flask containing sodium hydroxide solution, mix and stir until completely dissolved. Then add a solution of p-toluenesulfonyl chloride dissolved in acetonitrile dropwise into the flask, stir at a constant temperature for 2 hours, stop stirring, and allow to cool to room temperature.

[0009] (4) filtering the solution and washing it with deionized water, collecting and drying it to obtain an intermediate product;

[0010] (5) Add chitosan and 1-allylimidazole to the flask containing the acetic acid solution, mix and stir until the chitosan and 1-allylimidazole are completely dissolved. Dissolve the intermediate product obtained in step (4) in the DMF solution, mix and stir until it is completely dissolved. Then add the dissolved solution dropwise to the flask, stir at a constant temperature for 18-24 hours, stop heating, and cool to room temperature;

[0011] (6) Add the solution obtained in step (5) dropwise into the flask containing liquid paraffin and Span80, and react for 2-2.5 hours under constant temperature mechanical stirring. Then add the glutaraldehyde solution dropwise into the flask, and react for 2-2.5 hours under constant temperature mechanical stirring. Stop heating and cool to room temperature.

[0012] (7) Centrifuging the emulsion obtained in step (6), then washing the centrifuged product with petroleum ether and isopropanol in sequence, collecting and drying to obtain a modified chitosan double-container microsphere corrosion inhibitor.

[0013] Furthermore, the isothermal reaction temperature in step (1) is 50-60°C.

[0014] Furthermore, the molar ratio of benzotriazole:β-cyclodextrin:p-toluenesulfonyl chloride:sodium hydroxide is (0.5-1):(0.5-1):(0.5-1):1.

[0015] Furthermore, the isothermal reaction temperature in step (3) is -2-0°C.

[0016] Furthermore, the molar ratio of chitosan:1-allylimidazole:intermediate product is (5-5.5):(0.5-1):1.

[0017] Furthermore, the isothermal reaction temperature in step (5) is 95-100°C.

[0018] Furthermore, the volume ratio of the solution: liquid paraffin: glutaraldehyde is (2.5-3): (9.5-10): 1.

[0019] Furthermore, the isothermal reaction temperature in step (6) is 40-50°C.

[0020] The existing chitosan microsphere container preparation technology is to directly introduce a cross-linking agent to chemically modify the active amino groups on the chitosan molecular chain to obtain a single container system such as chitosan Schiff base microspheres. The present invention is different from this in that a second container is continuously introduced on the active amino groups of chitosan during the modification process. First, a mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin loaded with BTA is synthesized to generate an intermediate, and then the cyclodextrin is introduced into the chitosan molecular chain through the reaction of p-toluenesulfonyl and amino groups, and then a double container loading system is prepared while loading the main agent 1-allylimidazole by means of an emulsification cross-linking method. The container automatically locates the corrosion area, and the released corrosion inhibitor molecules and the heteroatoms in the chitosan molecular structure chelate with the metal surface, thereby forming a protective film to reduce the degree of surface corrosion. Through experimental analysis, it can be seen that the double container corrosion inhibition system exhibits excellent corrosion resistance in a sodium chloride solution saturated with carbon dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The synthetic route of the modified chitosan microsphere double container corrosion inhibitor of the embodiment of the present invention is shown in FIG.

[0022] Figure 2 This is an infrared characterization image of the modified chitosan microsphere double-container corrosion inhibitor according to an embodiment of the present invention.

[0023] Figure 3 This is a scanning electron microscope morphology image of the modified chitosan microsphere double container corrosion inhibitor of Example 1 of the present invention.

[0024] Figure 4 This is a scanning electron microscope morphology image of the modified chitosan microsphere double container corrosion inhibitor of Example 2 of the present invention.

[0025] Figure 5 This is a scanning electron microscope morphology image of the modified chitosan microsphere double container corrosion inhibitor of Example 3 of the present invention.

[0026] Figure 6 This is a scanning electron microscope morphology image of the modified chitosan microsphere double container corrosion inhibitor of Example 4 of the present invention.

[0027] Figure 7 This is the SEM characterization picture of N80 after corrosion under the conditions of room temperature, 48h, 1Mpa CO2, and 3.5wt% sodium chloride solution in the hanging piece weight loss experiment.

[0028] Figure 8 This is a SEM characterization picture of N80 after adding 200 mg / L of the modified chitosan corrosion inhibitor of Example 1 under the conditions of room temperature, 48h, 1Mpa CO2, and 3.5wt% sodium chloride solution in the hanging piece weight loss experiment.

[0029] Fig. 9This is a SEM characterization picture of N80 after adding 200 mg / L of modified chitosan corrosion inhibitor of Example 2 under the conditions of room temperature, 48h, 1Mpa CO2, and 3.5wt% sodium chloride solution in the hanging piece weight loss experiment.

[0030] Fig.10 This is a SEM characterization picture of N80 after adding 200 mg / L of the modified chitosan corrosion inhibitor of Example 3 under the conditions of room temperature, 48h, 1Mpa CO2, and 3.5wt% sodium chloride solution in the hanging piece weight loss experiment.

[0031] Fig.11 This is a SEM characterization picture of N80 after adding 200 mg / L of modified chitosan corrosion inhibitor of Example 4 under the conditions of room temperature, 48h, 1Mpa CO2, and 3.5wt% sodium chloride solution in the hanging piece weight loss experiment. DETAILED DESCRIPTION

[0032] The present invention is further described below by specific implementation examples, so that those skilled in the art can understand the present invention. The following description is only a preferred embodiment of the present invention, and is not intended to limit the present invention in any other form. Any modification or equivalent change made according to the technical essence of the present invention still belongs to the scope of protection claimed by the present invention.

[0033] Preparation of modified chitosan microsphere double container corrosion inhibitor:

[0034] Example 1

[0035] (1) Weigh 0.4 g of benzotriazole (BTA) and dissolve it in a flask containing 4 ml of acetone solution. Mix and stir until BTA is completely dissolved. Weigh 4 g of β-cyclodextrin (β-CD) and dissolve it in 20 ml of deionized water. Mix and stir until BTA is evenly dispersed in the water. Then add it dropwise to the flask, stir and react at a constant temperature of 55°C for 2 hours, stop heating, and cool to room temperature. Filter the solution containing the product and wash it with anhydrous ethanol. Collect and dry it to obtain a powder.

[0036] (2) Weigh 2.0 g of powder and dissolve it in a flask containing 0.35 ml of sodium hydroxide solution (8 mol / L), and stir until the solution becomes clear. Then weigh 0.6 g of p-toluenesulfonyl chloride (PTSC) and dissolve it in 2 ml of acetonitrile solution, and stir until PTSC is completely dissolved. Then add it dropwise to the flask, stir and react at a constant temperature of -2°C for 2 hours, stop the reaction, and let it cool to room temperature. Filter the solution containing the product and wash it with deionized water, collect and dry it to obtain the intermediate product.

[0037] (3) Weigh 1g chitosan and 1g 1-allylimidazole and dissolve them in a flask containing 20ml acetic acid solution, mix and stir until chitosan and 1-allylimidazole are completely dissolved. Weigh 1.5g intermediate product and dissolve it in 5ml DMF solution, mix and stir until the intermediate product is completely dissolved. Then add the dissolved solution dropwise into the flask, stir at constant temperature for 20h, stop heating, cool to room temperature, and collect to obtain a reaction solution. Measure 15ml reaction solution and add it dropwise into a flask containing 40ml liquid paraffin and 2ml Span80, and stir mechanically at constant temperature for 2.5h at 45℃. Then add 3ml glutaraldehyde solution dropwise into the flask, stir mechanically at constant temperature for 2.5h at 45℃, stop heating, cool to room temperature, and collect to obtain a reaction emulsion. Centrifuge the emulsion, then wash the centrifuged product with petroleum ether and isopropanol in turn, collect and dry to obtain a modified chitosan double-container microsphere corrosion inhibitor.

[0038] Example 2

[0039] (1) Weigh 0.4 g of benzotriazole (BTA) and dissolve it in a flask containing 4 ml of acetone solution. Mix and stir until BTA is completely dissolved. Weigh 4 g of β-cyclodextrin (β-CD) and dissolve it in 20 ml of deionized water. Mix and stir until BTA is evenly dispersed in the water. Then add it dropwise to the flask, stir and react at a constant temperature of 55°C for 2 hours, stop heating, and cool to room temperature. Filter the solution containing the product and wash it with anhydrous ethanol. Collect and dry it to obtain a powder.

[0040] (2) Weigh 2.0 g of powder and dissolve it in a flask containing 0.35 ml of sodium hydroxide solution (8 mol / L), and stir until the solution becomes clear. Then weigh 0.6 g of p-toluenesulfonyl chloride (PTSC) and dissolve it in 2 ml of acetonitrile solution, and stir until PTSC is completely dissolved. Then add it dropwise to the flask, stir and react at a constant temperature of -2°C for 2 hours, stop the reaction, and let it cool to room temperature. Filter the solution containing the product and wash it with deionized water, collect and dry it to obtain the intermediate product.

[0041] (3) Weigh 1g chitosan and 1g 1-allylimidazole and dissolve them in a flask containing 20ml acetic acid solution, mix and stir until chitosan and 1-allylimidazole are completely dissolved. Weigh 1.5g intermediate product and dissolve it in 5ml DMF solution, mix and stir until the intermediate product is completely dissolved. Then add the dissolved solution dropwise into the flask, stir at constant temperature for 22h, stop heating, cool to room temperature, and collect to obtain a reaction solution. Measure 8ml reaction solution and add it dropwise into a flask containing 40ml liquid paraffin and 2ml Span80, and stir mechanically at constant temperature for 2h at 50℃. Then add 2ml glutaraldehyde solution dropwise into the flask, stir mechanically at constant temperature for 2h at 50℃, stop heating, cool to room temperature, and collect to obtain a reaction emulsion. Centrifuge the emulsion, then wash the centrifuged product with petroleum ether and isopropanol in turn, collect and dry to obtain a modified chitosan double-container microsphere corrosion inhibitor.

[0042] Example 3

[0043] (1) Weigh 1g of benzotriazole (BTA) and dissolve it in a flask containing 8ml of acetone solution. Mix and stir until BTA is completely dissolved. Weigh 10g of β-cyclodextrin (β-CD) in 20ml of deionized water and stir until BTA is evenly dispersed in the water. Then add it dropwise to the flask, stir and react at a constant temperature of 55℃ for 2h, stop heating, and cool to room temperature. Filter the solution containing the product and wash it with anhydrous ethanol, collect and dry it to obtain a powder.

[0044] (2) Weigh 2.0 g of powder and dissolve it in a flask containing 0.35 ml of sodium hydroxide solution (8 mol / L), and stir until the solution becomes clear. Then weigh 0.8 g of p-toluenesulfonyl chloride (PTSC) and dissolve it in 2.5 ml of acetonitrile solution, and stir until PTSC is completely dissolved. Then add it dropwise to the flask, stir and react at a constant temperature of 0°C for 2 hours, stop the reaction, and let it cool to room temperature. Filter the solution containing the product and wash it with deionized water, collect and dry it to obtain the intermediate product.

[0045] (2) Weigh 1g chitosan and 1.5g 1-allylimidazole and dissolve them in a flask containing 20ml acetic acid solution, mix and stir until chitosan and 1-allylimidazole are completely dissolved. Weigh 2g intermediate product and dissolve it in 5ml DMF solution, mix and stir until the intermediate product is completely dissolved. Then add the dissolved solution dropwise into the flask, stir at constant temperature for 20h, stop heating, cool to room temperature, and collect to obtain a reaction solution. Measure 15ml reaction solution and add it dropwise into a flask containing 40ml liquid paraffin and 2ml Span80, and stir mechanically at constant temperature for 2.5h at 45℃. Then add 3ml glutaraldehyde solution dropwise into the flask, stir mechanically at constant temperature for 2.5h at 45℃, stop heating, cool to room temperature, and collect to obtain a reaction emulsion. Centrifuge the emulsion, then wash the centrifuged product with petroleum ether and isopropanol in turn, collect and dry to obtain a modified chitosan double-container microsphere corrosion inhibitor.

[0046] Example 4

[0047] (1) Weigh 1g of benzotriazole (BTA) and dissolve it in a flask containing 8ml of acetone solution. Mix and stir until BTA is completely dissolved. Weigh 10g of β-cyclodextrin (β-CD) in 20ml of deionized water and stir until BTA is evenly dispersed in the water. Then add it dropwise to the flask, stir and react at a constant temperature of 55℃ for 2h, stop heating, and cool to room temperature. Filter the solution containing the product and wash it with anhydrous ethanol, collect and dry it to obtain a powder.

[0048] (2) Weigh 2.0 g of powder and dissolve it in a flask containing 0.35 ml of sodium hydroxide solution (8 mol / L), and stir until the solution becomes clear. Then weigh 0.8 g of p-toluenesulfonyl chloride (PTSC) and dissolve it in 2.5 ml of acetonitrile solution, and stir until PTSC is completely dissolved. Then add it dropwise to the flask, stir and react at a constant temperature of 0°C for 2 hours, stop the reaction, and let it cool to room temperature. Filter the solution containing the product and wash it with deionized water, collect and dry it to obtain the intermediate product.

[0049] (3) Weigh 1g chitosan and 1.5g 1-allylimidazole and dissolve them in a flask containing 20ml acetic acid solution, mix and stir until chitosan and 1-allylimidazole are completely dissolved. Weigh 2g intermediate product and dissolve it in 5ml DMF solution, mix and stir until the intermediate product is completely dissolved. Then add the dissolved solution dropwise into the flask, stir at constant temperature for 22h, stop heating, cool to room temperature, and collect to obtain a reaction solution. Measure 8ml reaction solution and add it dropwise into a flask containing 40ml liquid paraffin and 2ml Span80, and stir mechanically at constant temperature for 2h at 50℃. Then add 2ml glutaraldehyde solution dropwise into the flask, stir mechanically at constant temperature for 2h at 50℃, stop heating, cool to room temperature, and collect to obtain a reaction emulsion. Centrifuge the emulsion, then wash the centrifuged product with petroleum ether and isopropanol in turn, collect and dry to obtain a modified chitosan double-container microsphere corrosion inhibitor.

[0050] The prepared modified chitosan microsphere double container corrosion inhibitor molecule was tested by infrared spectroscopy. The results are as follows Figure 2 As shown (detection instrument used: ThermoScientific Nicolet IS50 Fourier transform infrared spectrometer from Thermo Fisher Scientific, USA);

[0051] Figure 2 1642cm -1 and 1156cm -1 The characteristic peak at 1660 cm-1 is attributed to the C=C stretching of the aromatic group and the S=O stretching of the sulfonyl group. -1 The characteristic peak at 1574 cm represents the stretching vibration of CN. -1 The obvious absorption peak at is attributed to the stretching vibration of C=N, which indicates that β-cyclodextrin is successfully grafted onto chitosan and the Schiff base reaction is successfully carried out.

[0052] The morphology of the prepared modified chitosan microsphere double container corrosion inhibitor molecules was observed by scanning electron microscopy. Figure 3 As shown (detection instrument used: Thermo Fisher Talos F200X field emission scanning transmission electron microscope, USA);

[0053] Figure 3 The microsphere products in the experiment had regular shapes, and their main sizes were between 15 μm and 20 μm, indicating that the microspheres were successfully prepared.

[0054] CO2 corrosion resistance test of modified chitosan microsphere double container corrosion inhibitor:

[0055] The anti-corrosion performance of the corrosion inhibitors of Examples 1-4 on N80 steel sheets was tested using the hanging plate method in a room temperature, 1Mpa CO2, 3.5wt% sodium chloride solution environment. The steps are as follows:

[0056] (1) Before the weight loss experiment, the steel sheet was degreased with acetone solution, and then cleaned with deionized water and anhydrous ethanol in sequence. The cleaned steel sheet was blown dry and wrapped with filter paper. It was placed in a desiccator and dried for 5 hours. The weight was then weighed with an electronic balance with an accuracy of 0.0001g.

[0057] (2) Measure 200 ml of deionized water and 100 ml of hydrochloric acid and pour them into a volumetric flask in sequence, then weigh 3.6 g of hexamethylenetetramine and add it to the volumetric flask, and then make up to 1000 ml with deionized water to prepare a rust removal solution;

[0058] (3) After cleaning the autoclave, first pour in an appropriate amount of 3.5wt% sodium chloride solution, then add the corrosion inhibitor and mix it evenly with the solution, assemble and fix the autoclave device. First, introduce CO2 gas into the autoclave for 1 hour to deoxygenate, and then continue to introduce CO2 to the pressure value required for the experiment, and open the autoclave after 48 hours;

[0059] (4) Take out the steel sheet from the reactor, place it in a beaker containing rust removal liquid and ultrasonicate it for 4 minutes, then wipe the corrosion products on the surface of the steel sheet with absorbent cotton. Then rinse off the residual liquid on the surface with clean water, soak it in a beaker containing anhydrous ethanol for 4 minutes for cleaning, and then place the steel sheet in a beaker containing acetone solution for cleaning. After the cleaned steel sheet is blown dry, wrap it with filter paper, place it in a dryer and dry it for 5 hours, and then weigh it again with an electronic balance with an accuracy of 0.0001g;

[0060] (5) The corrosion rate v of N80 steel sheet is calculated using the formula:

[0061]

[0062] Where: v——corrosion rate, mm / a; Δm——mass difference of steel sheet before and after corrosion, g; S——surface area of ​​steel sheet, cm 2 ; ρ——carbon steel density, g / cm 3 ; t——corrosion reaction time, h.

[0063] The corrosion inhibition efficiency η of the corrosion inhibitor is calculated using the formula:

[0064]

[0065] Where: v0 is the corrosion rate without corrosion inhibitor (mm / a); v i is the corrosion rate after adding corrosion inhibitor, mm / a.

[0066] The experimental results of each group are the average values ​​of corrosion rate and corrosion efficiency obtained from 3 steel sheets.

[0067] Table 1 Corrosion inhibition performance of modified chitosan microsphere double container corrosion inhibitor (Examples 1-4) on N80 steel sheet at room temperature, 48h, 1Mpa CO2, 3.5wt% sodium chloride solution environment

[0068]

[0069] As shown in Table 1, the prepared modified chitosan microsphere double container corrosion inhibitor has excellent anti-corrosion performance for N80 steel in a CO2 environment. Analysis of the weight loss test data shows that the corrosion rate of the steel sheet can be reduced after adding the corrosion inhibitor compared with the blank group. With the increase of the corrosion inhibitor concentration, the corrosion inhibition efficiency further increases. When the corrosion inhibitor concentration is 200 mg / L, the corrosion inhibition efficiency is higher than 90%. In addition, scanning electron microscopy was performed on the blank sample and the steel sheet with 200 mg / L of corrosion inhibitor added (Examples 1-4). Figure 3-7 From the surface morphology diagram, it can be seen that obvious corrosion pits appear on the surface of the blank sample steel sheet, and the surface roughness of the sample is relatively large. The surface of the steel sheet of Examples 1-4 with the addition of corrosion inhibitor is smoother, with fewer corrosion pits and a reduced degree of corrosion, indicating that the modified chitosan microsphere double-container corrosion inhibitor prepared by the present invention has an excellent corrosion inhibition effect on N80 steel in a CO2 environment.

Claims

1. A method for preparing a modified chitosan microsphere double-container corrosion inhibitor, characterized in that: The following steps are involved: (1) Dissolve benzotriazole (BTA) in acetone solution, mix and stir until BTA is completely dissolved. Then add the dissolved solution into a flask containing an aqueous solution of β-cyclodextrin (β-CD), and stir at a constant temperature for 2 hours; (2) filtering the solution and washing it with deionized water, collecting and drying it to obtain an intermediate product; (3) Add the intermediate product obtained in step (2) into a flask containing sodium hydroxide solution, mix and stir until completely dissolved. Then add a solution of p-toluenesulfonyl chloride dissolved in acetonitrile dropwise into the flask, stir at a constant temperature for 2 hours, stop stirring, and allow to cool to room temperature. (4) filtering the solution and washing it with deionized water, collecting and drying it to obtain an intermediate product; (5) Add chitosan and 1-allylimidazole to the flask containing the acetic acid solution, mix and stir until the chitosan and 1-allylimidazole are completely dissolved. Dissolve the intermediate product obtained in step (4) in the DMF solution, mix and stir until it is completely dissolved. Then add the dissolved solution dropwise to the flask, stir at a constant temperature for 18-24 hours, stop heating, and cool to room temperature; (6) Add the solution obtained in step (5) dropwise into the flask containing liquid paraffin and Span80, and react for 2-2.5 hours under constant temperature mechanical stirring. Then add the glutaraldehyde solution dropwise into the flask, and react for 2-2.5 hours under constant temperature mechanical stirring. Stop heating and cool to room temperature. (7) Centrifuging the emulsion obtained in step (6), then washing the centrifuged product with petroleum ether and isopropanol in sequence, collecting and drying to obtain a modified chitosan double-container microsphere corrosion inhibitor.

2. The method for preparing a modified chitosan microsphere double container corrosion inhibitor according to claim 1, characterized in that: The isothermal reaction temperature in step (1) is 50-60°C.

3. The method for preparing a modified chitosan microsphere double container corrosion inhibitor according to claim 1, characterized in that: The molar ratio of benzotriazole:β-cyclodextrin:p-toluenesulfonyl chloride:sodium hydroxide is (0.5-1):(0.5-1):(0.5-1):

1.

4. The method for preparing a modified chitosan microsphere double-container corrosion inhibitor according to claim 1, characterized in that: The isothermal reaction temperature in step (3) is -2-0°C.

5. The method for preparing a modified chitosan microsphere double container corrosion inhibitor according to claim 1, characterized in that: The molar ratio of chitosan:1-allylimidazole:intermediate product is (5-5.5):(0.5-1):

1.

6. The method for preparing a modified chitosan microsphere double-container corrosion inhibitor according to claim 1, characterized in that: The isothermal reaction temperature in step (5) is 95-100°C.

7. The method for preparing a modified chitosan microsphere double-container corrosion inhibitor according to claim 1, characterized in that: The volume ratio of the solution: liquid paraffin: glutaraldehyde is (2.5-3): (9.5-10):

1.

8. The method for preparing a modified chitosan microsphere double-container corrosion inhibitor according to claim 1, characterized in that: The isothermal reaction temperature in step (6) is 40-50°C.

Citation Information

Cited By

  • Environment-friendly sewage treatment flocculant and preparation method thereof

    CN119285056A