Ceramic fire-resistant silicone rubber foaming belt and preparation method thereof
Through the preparation of modified silicone rubber and the uniform dispersion technology of fillers, the problem of limited strength increase of the ceramic layer after calcining of ceramic silicone rubber is solved, and the strength increase and mechanical properties of the ceramic layer are improved.
Patent Information
- Application Number
- CN202410938224.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
When existing ceramic silicone rubber uses magnesium hydroxide and aluminum hydroxide as inorganic fillers, the strength improvement of the ceramic layer after calcination is limited, and the uneven distribution and poor compatibility of the fillers limit the strength improvement of the ceramic layer.
Using modified silicone rubber as the main material, by grafting a polyamino structure on the hydrogen-containing silicone rubber, and adding aluminum salts and magnesium salts under alkaline conditions, the magnesium ions and aluminum ions are evenly dispersed to form magnesium hydroxide and hydrogen Alumina, combined with methyl vinyl silicone rubber, is cross-linked to form a network structure to ensure uniform dispersion, and fillers such as fumed silica, muscovite, and glass powder are introduced to improve mechanical properties and flame retardant properties.
It achieves the improvement of the strength of the ceramic layer and the uniform dispersion of fillers, enhances the strength of the calcined ceramic layer, and improves the mechanical and flame retardant properties of ceramic silicone rubber through the combination of various fillers.
Smart Images

Figure BDA0004942109780000101 
Figure BDA0004942109780000111 
Figure BDA0004942109780000112
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic silicone rubber, and in particular relates to a ceramic fire-resistant silicone rubber foaming belt and a preparation method thereof. Background Art
[0002] Silicone rubber is a material with good insulation performance and flame retardancy, and is widely used in refractory materials. However, in the event of a fire, silicone rubber will turn into powder under the burning of the flame and can hardly maintain its strength, which greatly reduces its fire protection performance. In order to solve the above problems, people have found that adding some inorganic fillers to silicone rubber, making it melt under high temperature conditions, and then forming a dense ceramic layer can effectively solve the above problems. Therefore, ceramic silicone rubber has received more and more attention.
[0003] Ceramic silicone rubber generally uses vinyl silicone rubber as the main material, and adds flame retardants, ceramic fillers, fluxing agents, crosslinking agents, etc. to the vinyl silicone rubber. At high temperatures, the silicone rubber will decompose to produce silicon dioxide, which will react with the molten inorganic filler to form a hard and dense ceramic layer. However, with the development of society and higher safety performance considerations, people have put forward higher requirements for the strength of the ceramic layer after calcination. After research, it was found that when magnesium hydroxide and strong alumina inorganic fillers are added to silicone rubber, they will form MgAl2Si4O with silicon in the silicone rubber system at high temperatures. 12 Crystallization can effectively improve the strength of the ceramic layer after calcination. However, due to the fact that magnesium hydroxide and aluminum hydroxide are prone to agglomeration when added as fillers, they are unevenly distributed in the silicone rubber system and have poor compatibility with the silicone rubber system, the MgAl2Si4O 12 More crystals are formed, which in turn limits the improvement of the strength of the ceramic layer after calcination. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect of the existing ceramic silicone rubber that the strength of the ceramic layer after calcination is limited when magnesium hydroxide and aluminum hydroxide are used as inorganic fillers, and further provide a ceramic refractory silicone rubber foam belt and a preparation method thereof.
[0005] In order to solve the above problems, the scheme of the present invention is as follows:
[0006] A ceramic fire-resistant silicone rubber, comprising the following raw materials in parts by weight:
[0007] 50-70 parts of methyl vinyl silicone rubber with a vinyl content of 0.04-0.06%, 30-50 parts of methyl vinyl silicone rubber with a vinyl content of 0.2-0.24%, 20-35 parts of modified silicone rubber, 35-45 parts of fumed silica, 30-40 parts of muscovite, 5-15 parts of glass powder, 3-8 parts of zinc borate, 0.02-0.08 parts of the first catalyst, 1-4 parts of hydrogenated silicone oil, and 1-4 parts of vulcanizing agent.
[0008] Preferably, the preparation method of the modified silicone rubber comprises the following steps:
[0009] 1) mixing hydrogenated silicone rubber, a second catalyst, trichlorovinyl silane and a first organic solvent and reacting them, adding sodium amide after the reaction, continuing the reaction, washing after the reaction, and drying to obtain amino-modified hydrogenated silicone rubber;
[0010] 2) The amino-modified hydrogenated silicone rubber prepared in step 1), the second organic solvent and water are mixed, ultrasonically dispersed, and then aluminum salt and magnesium salt are added to the ultrasonic dispersion, stirred, and then the pH of the mixed solution is adjusted to 10-13, and the stirring is continued, allowed to stand, filtered, the filter cake is washed with water, and dried to obtain the modified silicone rubber.
[0011] Preferably, the mass ratio of the hydrogenated silicone rubber, the second catalyst, trichlorovinyl silane, the first organic solvent and sodium amide is 1: (0.05-0.2): (0.3-0.8): (10-20): (0.32-0.4).
[0012] Preferably, the viscosity of the hydrogenated silicone rubber is 2000-3000 mPa·s; the hydrogenated silicone rubber in the present invention is an existing product, which can be obtained commercially or prepared by an existing method, for example, vinyl-terminated polydimethylsiloxane, hydrogenated silicone oil, and Pt catalyst (the mass ratio of vinyl-terminated polydimethylsiloxane, hydrogenated silicone oil and Pt catalyst is 100:3.5:0.2) are mixed, heated at 60° C. for reaction for 10 hours, and after the reaction is completed, washed with ethanol and water in sequence, and dried to obtain the hydrogenated silicone rubber.
[0013] The second catalyst is catalyst Pt, the first organic solvent is selected from toluene and anhydrous ethanol, and the mass ratio of toluene to anhydrous ethanol is 10:(1-3);
[0014] The amount of aluminum salt added is 40-65% of the mass of hydrogen-containing silicone rubber, and the amount of magnesium salt added is 15-30% of the mass of hydrogen-containing silicone rubber;
[0015] The second organic solvent is ethanol, and the mass ratio of the second organic solvent to water is (0.2-0.6):1;
[0016] In step 2), the amount of the second organic solvent added is 4-7 times the mass of the hydrogen-containing silicone rubber.
[0017] Preferably, in step 1), the reaction temperature is 60-75°C, the reaction time is 5-15h, and the continued reaction time is 1-5h;
[0018] The washing step in step 1) is performed using ethanol and water;
[0019] In step 2), the stirring temperature is 55-70°C, the stirring time is 0.5-3h, the stirring temperature is continued to be 55-70°C, the stirring time is continued to be 1-3h, the standing temperature is 55-70°C, and the standing time is 3-8h;
[0020] The ultrasonic dispersion time is 0.5-1.5h, and the ultrasonic power is 200-500W;
[0021] The pH value of the mixed solution is adjusted to 10-13 using a sodium hydroxide solution with a mass fraction of 8-15%;
[0022] The aluminum salt is selected from aluminum chloride, and the magnesium salt is selected from magnesium chloride.
[0023] Preferably, the first catalyst is composed of diethyl phthalate platinum complex and Raney nickel, and the mass ratio of diethyl phthalate platinum complex to Raney nickel is (1.5-2.5):1;
[0024] The hydrogen content of the hydrogen-containing silicone oil is 0.1-0.25%, and the viscosity is 100-200 mPa·s;
[0025] The vulcanizing agent is selected from bis(2,4-dichlorobenzoyl) peroxide.
[0026] In the present invention, the vinyl content of the methyl vinyl silicone rubber with a vinyl content of 0.04-0.06% and the methyl vinyl silicone rubber with a vinyl content of 0.2-0.24% refers to the molar content. The molecular weight of the methyl vinyl silicone rubber with a vinyl content of 0.04-0.06% and the methyl vinyl silicone rubber with a vinyl content of 0.2-0.24% used in the present invention is selected to be 550,000-750,000.
[0027] The present invention also provides a method for preparing the ceramic refractory silicone rubber, comprising the following steps:
[0028] Methyl vinyl silicone rubber with a vinyl content of 0.04-0.06%, methyl vinyl silicone rubber with a vinyl content of 0.2-0.24%, modified silicone rubber and fumed silica are mixed, and muscovite, glass powder, zinc borate, a first catalyst, and hydrogen-containing silicone oil are added after the mixing is completed and the mixing is continued. After the mixing is completed, vacuum is drawn, and then a desulfurizer is added and mixed again, and vulcanization is performed to obtain the ceramicized refractory silicone rubber.
[0029] Preferably, the mixing temperature is 80-100°C, the mixing time is 30-60min, the continued mixing temperature is 90-110°C, and the continued mixing time is 1-3h;
[0030] The vacuum operation temperature is 120-150℃, and the vacuum time is 20-40min;
[0031] The mixing time is 20-40 minutes again;
[0032] The vulcanization temperature is 160-180°C and the vulcanization time is 1-3h.
[0033] The present invention also provides a ceramic fire-resistant silicone rubber foam belt, comprising the ceramic fire-resistant silicone rubber described above;
[0034] Preferably, the ceramicized refractory silicone rubber foam belt also includes glass cloth.
[0035] The present invention also provides a method for preparing the ceramicized refractory silicone rubber foam tape, comprising the following steps: obtaining the ceramicized refractory silicone rubber and glass cloth through a calendering process.
[0036] The technical solution of the present invention has the following advantages:
[0037] The ceramic fire-resistant silicone rubber provided by the invention adopts methyl vinyl silicone rubber with a vinyl content of 0.04-0.06% and methyl vinyl silicone rubber with a vinyl content of 0.2-0.24% as main materials, and introduces modified silicone rubber on this basis. The preparation of the modified silicone rubber adopts hydrogen-containing silicone rubber as the main material, and polyamino structures are grafted on the hydrogen-containing silicone rubber by trichlorovinyl silane and sodium amide to obtain amino-modified hydrogen-containing silicone rubber, and then the amino-modified hydrogen-containing silicone rubber is dispersed, and aluminum salt and magnesium salt are added. Magnesium ions and aluminum ions are uniformly dispersed on the surface of the hydrogen-containing silicone rubber under the chelation action of amino groups, and magnesium hydroxide and aluminum hydroxide are subsequently formed under alkaline conditions. After that, the modified silicone rubber is further cross-linked with the methyl vinyl silicone rubber to form a network structure due to its active hydrogen, and the magnesium hydroxide and aluminum hydroxide are uniformly confined in the grid structure to achieve the purpose of uniform dispersion. The invention can better realize the dispersion of magnesium hydroxide and aluminum hydroxide by adding specific modified silicone rubber, and increase their compatibility, which is conducive to the formation of more MgAl2Si4O 12 In addition, the present invention introduces fillers such as fumed silica, muscovite, glass powder, zinc borate, and hydrogen-containing silicone oil into the silicone rubber system, and the combination of these materials effectively improves the mechanical properties and flame retardant properties of the ceramic silicone rubber. DETAILED DESCRIPTION
[0038] The following examples are provided for further understanding of the present invention, but are not intended to limit the best mode of implementation and do not limit the scope of protection of the present invention.
[0039] The experimental steps or conditions not specified in the following embodiments of the present invention can be implemented according to the conventional experimental steps and conditions used in the existing literature in the field. The reagents or instruments used without specifying the manufacturer are all conventional reagents or instruments that can be purchased commercially.
[0040] Example 1
[0041] This embodiment provides a method for preparing ceramic refractory silicone rubber, comprising the following steps:
[0042] 50kg of methyl vinyl silicone rubber with a vinyl content of 0.05%, 30kg of methyl vinyl silicone rubber with a vinyl content of 0.2%, 20kg of modified silicone rubber and 40kg of fumed silica are mixed in a kneader at a mixing temperature of 90°C and a mixing time of 60min. After the mixing is completed, 30kg of muscovite, 10kg of glass powder, 5kg of zinc borate, 0.04kg of diethyl phthalate platinum complex, 0.02kg of Raney nickel and 2kg of hydrogen-containing silicone oil (with a hydrogen content of 0.2% and a viscosity of 150mPa·s) are added and the mixing is continued at a mixing temperature of 100°C and a mixing time of 2h. After the mixing is completed, vacuum is drawn at 140°C for 40min, and then 2kg of bis(2,4-dichlorobenzoyl) peroxide is added on an open mill and mixed for 20min. The mixture is vulcanized at 170°C for 1.5h to obtain the ceramicized refractory silicone rubber.
[0043] The preparation method of the modified silicone rubber comprises the following steps:
[0044] 1) 1 kg of hydrogenated silicone rubber (viscosity of 3000 mPa·s), 0.1 kg of catalyst Pt, 0.5 kg of trichlorovinyl silane, 10 kg of toluene and 1 kg of anhydrous ethanol were mixed and reacted at a temperature of 70°C for 10 h. After the reaction, 0.38 kg of sodium amide was added and the reaction was continued for 3 h. After the reaction was completed, it was washed with ethanol and water in turn and dried to obtain amino-modified hydrogenated silicone rubber;
[0045] 2) The amino-modified hydrogenated silicone rubber prepared in step 1), 5 kg of ethanol and 10 kg of water were mixed, and ultrasonically dispersed for 1.0 h at an ultrasonic power of 400 W. Then, 5 mol of AlCl3 and 2.5 mol of MgCl2 were added to the ultrasonic dispersion, and the mixture was stirred at 60° C. for 1.0 h. Then, a 10% by mass sodium hydroxide solution was added to adjust the pH of the mixture to 12. The mixture was further stirred at 60° C. for 1.5 h, and then allowed to stand at 60° C. for 6 h. The mixture was filtered, the filter cake was washed with water, and dried to obtain the modified silicone rubber, wherein the mass of aluminum hydroxide in the modified silicone rubber accounted for 12.5% of the total mass of the modified silicone rubber, and the mass of magnesium hydroxide accounted for 4.2% of the total mass of the modified silicone rubber.
[0046] Example 2
[0047] This embodiment provides a method for preparing ceramic refractory silicone rubber, comprising the following steps:
[0048] 50kg of methyl vinyl silicone rubber with a vinyl content of 0.05%, 35kg of methyl vinyl silicone rubber with a vinyl content of 0.2%, 25kg of modified silicone rubber and 50kg of fumed silica are mixed in a kneader at a mixing temperature of 90°C and a mixing time of 120min. After the mixing is completed, 35kg of muscovite, 5kg of glass powder, 4kg of zinc borate, 0.03kg of diethyl phthalate platinum complex, 0.02kg of Raney nickel and 1.5kg of hydrogen-containing silicone oil (with a hydrogen content of 0.2% and a viscosity of 150mPa·s) are added and the mixing is continued at a mixing temperature of 100°C and a mixing time of 2h. After the mixing is completed, vacuum is drawn at 130°C for 40min, and then 2kg of bis(2,4-dichlorobenzoyl) peroxide is added on an open mill and mixed for 20min. The mixture is vulcanized at 160°C for 1.5h to obtain the ceramicized refractory silicone rubber.
[0049] The preparation method of the modified silicone rubber comprises the following steps:
[0050] 1) 1 kg of hydrogenated silicone rubber (viscosity of 3000 mPa·s), 0.1 kg of catalyst Pt, 0.5 kg of trichlorovinyl silane, 15 kg of toluene and 1 kg of anhydrous ethanol were mixed and reacted at a temperature of 65°C for 10 h. After the reaction, 0.4 kg of sodium amide was added and the reaction was continued for 3 h. After the reaction was completed, the rubber was washed with ethanol and water in turn and dried to obtain amino-modified hydrogenated silicone rubber;
[0051] 2) The amino-modified hydrogenated silicone rubber prepared in step 1) is mixed with 5 kg of ethanol and 10 kg of water, and ultrasonically dispersed for 1.5 h at an ultrasonic power of 400 W, and then 4.5 mol of AlCl3 and 3 mol of MgCl2 are added to the ultrasonic dispersion, and stirred at 60° C. for 1.0 h, and then a 10% by mass sodium hydroxide solution is added to adjust the pH of the mixed solution to 12, and the mixture is further stirred at 60° C. for 1.5 h, and then allowed to stand at 60° C. for 6 h, filtered, and the filter cake is washed with water and dried to obtain the modified silicone rubber, wherein the mass of aluminum hydroxide in the modified silicone rubber accounts for 8.5% of the total mass of the modified silicone rubber, and the mass of magnesium hydroxide accounts for 4.5% of the total mass of the modified silicone rubber.
[0052] Example 3
[0053] This embodiment provides a method for preparing ceramic refractory silicone rubber, comprising the following steps:
[0054] 50kg of methyl vinyl silicone rubber with a vinyl content of 0.05%, 40kg of methyl vinyl silicone rubber with a vinyl content of 0.2%, 30kg of modified silicone rubber and 50kg of fumed silica were mixed in a kneader at a mixing temperature of 90°C and a mixing time of 120min. After the mixing was completed, 40kg of muscovite, 5kg of glass powder, 4kg of zinc borate, 0.03kg of diethyl phthalate platinum complex, 0.02kg of Raney nickel and 2.0kg of hydrogen-containing silicone oil (with a hydrogen content of 0.2% and a viscosity of 150mPa·s) were added and the mixing was continued at a mixing temperature of 100°C and a mixing time of 2h. After the mixing was completed, vacuum was drawn at 130°C for 60min, and then 2.5kg of bis(2,4-dichlorobenzoyl) peroxide was added on an open mill and mixed for 20min. The mixture was vulcanized at 160°C for 1.5h to obtain the ceramicized refractory silicone rubber.
[0055] The preparation method of the modified silicone rubber comprises the following steps:
[0056] 1) 1 kg of hydrogenated silicone rubber (viscosity of 3000 mPa·s), 0.1 kg of catalyst Pt, 0.5 kg of trichlorovinyl silane, 15 kg of toluene and 1 kg of anhydrous ethanol were mixed and reacted at a temperature of 65°C for 10 hours. After the reaction, 0.4 kg of sodium amide was added and the reaction was continued for 4 hours. After the reaction was completed, it was washed with ethanol and water in turn and dried to obtain amino-modified hydrogenated silicone rubber;
[0057] 2) The amino-modified hydrogenated silicone rubber prepared in step 1), 5 kg of ethanol and 10 kg of water were mixed, and ultrasonically dispersed for 1.5 h at an ultrasonic power of 400 W. Then, 4.5 mol of AlCl3 and 3 mol of MgCl2 were added to the ultrasonic dispersion, and the mixture was stirred at 60° C. for 1.5 h. Then, a 10% by mass sodium hydroxide solution was added to adjust the pH of the mixture to 12. The mixture was further stirred at 60° C. for 2 h, and then allowed to stand at 60° C. for 6 h. The mixture was filtered, the filter cake was washed with water, and dried to obtain the modified silicone rubber, wherein the mass of aluminum hydroxide in the modified silicone rubber accounted for 8.8% of the total mass of the modified silicone rubber, and the mass of magnesium hydroxide accounted for 4.7% of the total mass of the modified silicone rubber.
[0058] Example 4
[0059] This embodiment provides a method for preparing ceramic refractory silicone rubber, comprising the following steps:
[0060] 50kg of methyl vinyl silicone rubber with a vinyl content of 0.05%, 40kg of methyl vinyl silicone rubber with a vinyl content of 0.2%, 28kg of modified silicone rubber and 48kg of fumed silica were mixed in a kneader at a mixing temperature of 90°C and a mixing time of 80min. After the mixing was completed, 35kg of muscovite, 5kg of glass powder, 4kg of zinc borate, 0.04kg of diethyl phthalate platinum complex, 0.01kg of Raney nickel and 2.0kg of hydrogen-containing silicone oil (with a hydrogen content of 0.2% and a viscosity of 150mPa·s) were added and the mixing was continued at a mixing temperature of 100°C and a mixing time of 2h. After the mixing was completed, vacuum was drawn at 130°C for 60min, and then 2.5kg of bis(2,4-dichlorobenzoyl) peroxide was added on an open mill and mixed for 20min. The mixture was vulcanized at 160°C for 1.5h to obtain the ceramicized refractory silicone rubber.
[0061] The preparation method of the modified silicone rubber comprises the following steps:
[0062] 1) 1 kg of hydrogenated silicone rubber (viscosity of 3000 mPa·s), 0.1 kg of catalyst Pt, 0.5 kg of trichlorovinyl silane, 15 kg of toluene and 1 kg of anhydrous ethanol were mixed and reacted at a temperature of 65°C for 10 h. After the reaction, 0.4 kg of sodium amide was added and the reaction was continued for 6 h. After the reaction was completed, the mixture was washed with ethanol and water in turn and dried to obtain amino-modified hydrogenated silicone rubber;
[0063] 2) The amino-modified hydrogenated silicone rubber prepared in step 1) is mixed with 6 kg of ethanol and 10 kg of water, and ultrasonically dispersed for 2.0 h at an ultrasonic power of 400 W. Then, 4.5 mol of AlCl3 and 3 mol of MgCl2 are added to the ultrasonic dispersion, and stirred at 60° C. for 1.0 h. Then, a 10% by mass sodium hydroxide solution is added to adjust the pH of the mixed solution to 13. The mixture is further stirred at 60° C. for 1.5 h, and then allowed to stand at 60° C. for 10 h. The mixture is filtered, the filter cake is washed with water, and dried to obtain the modified silicone rubber, wherein the mass of aluminum hydroxide in the modified silicone rubber accounts for 9.2% of the total mass of the modified silicone rubber, and the mass of magnesium hydroxide accounts for 4.9% of the total mass of the modified silicone rubber.
[0064] Comparative Example 1
[0065] This comparative example provides a method for preparing a ceramic refractory silicone rubber, comprising the following steps:
[0066] 70kg of methyl vinyl silicone rubber with a vinyl content of 0.05%, 30kg of methyl vinyl silicone rubber with a vinyl content of 0.2% and 40kg of fumed silica are mixed in a kneader at a mixing temperature of 90°C and a mixing time of 60min. After the mixing is completed, 30kg of muscovite, 10kg of glass powder, 5kg of zinc borate, 0.04kg of diethyl phthalate platinum complex, 0.02kg of Raney nickel and 2kg of hydrogen-containing silicone oil (with a hydrogen content of 0.2% and a viscosity of 150mPa·s) are added and the mixing is continued at a mixing temperature of 100°C and a mixing time of 2h. After the mixing is completed, vacuum is drawn at 140°C for 40min, and then 2kg of bis(2,4-dichlorobenzoyl) peroxide is added on an open mill and mixed for 20min. The mixture is vulcanized at 170°C for 1.5h to obtain the ceramicized refractory silicone rubber.
[0067] Comparative Example 2
[0068] This comparative example provides a method for preparing a ceramic refractory silicone rubber, comprising the following steps:
[0069] 50kg of methyl vinyl silicone rubber with a vinyl content of 0.05%, 30kg of methyl vinyl silicone rubber with a vinyl content of 0.2%, 16.66kg of amino-modified hydrogenated silicone rubber, 2.5kg of aluminum hydroxide, 0.84kg of magnesium hydroxide and 40kg of fumed silica were mixed in a kneader at a mixing temperature of 90°C for 60 minutes. After the mixing was completed, 30kg of muscovite, 10kg of glass powder, 5kg of zinc borate, and 0.04kg of o-phthalate were added. Diethyl diformate platinum complex, 0.02kg Raney nickel, and 2kg hydrogen-containing silicone oil (hydrogen content of 0.2%, viscosity of 150mPa·s) are continuously mixed at a mixing temperature of 100°C and a mixing time of 2h. After the mixing is completed, vacuum is drawn at 140°C for 40min, and then 2kg bis(2,4-dichlorobenzoyl) peroxide is added on an open mill and mixed for 20min, and then vulcanized at 170°C for 1.5h to obtain the ceramicized refractory silicone rubber.
[0070] The preparation method of the amino-modified hydrogenated silicone rubber comprises the following steps:
[0071] 1 kg of hydrogenated silicone rubber (viscosity of 3000 mPa·s), 0.1 kg of catalyst Pt, 0.5 kg of trichlorovinyl silane, 10 kg of toluene and 1 kg of anhydrous ethanol were mixed and reacted at 70°C for 10 h. After the reaction, 0.38 kg of sodium amide was added and the reaction was continued for 3 h. After the reaction was completed, it was washed with ethanol and water in turn and dried to obtain amino-modified hydrogenated silicone rubber.
[0072] Comparative Example 3
[0073] This comparative example provides a method for preparing a ceramicized fire-resistant silicone rubber, which is different from Example 1 in that the method for preparing the modified silicone rubber comprises the following steps:
[0074] 1 kg of hydrogenated silicone rubber (viscosity of 3000 mPa·s), 5 kg of ethanol and 10 kg of water were mixed and ultrasonically dispersed for 1.0 h at an ultrasonic power of 400 W. Then, 5 mol of AlCl3 and 2.5 mol of MgCl2 were added to the ultrasonic dispersion and stirred at 60° C. for 1.0 h. Then, a 10% by mass sodium hydroxide solution was added to adjust the pH of the mixture to 12. The mixture was stirred at 60° C. for 1.5 h and then allowed to stand at 60° C. for 6 h. The mixture was filtered, the filter cake was washed with water and dried to obtain the modified silicone rubber.
[0075] Test Example 1
[0076] The mechanical properties of the ceramic refractory silicone rubber prepared in the above embodiment were tested according to GB / T 528-2009 standard;
[0077] The flame retardant performance is tested according to GB / T11020-2005;
[0078] The test results are shown in Table 1.
[0079] Table 1
[0080]
[0081]
[0082] Test Example 2
[0083] The ceramicized refractory silicone rubber prepared in the above examples and comparative examples was made into test specimens with a size of 100*30*3 mm, and calcined in a muffle furnace at 800° C. for 15 min in an air atmosphere to test the bending resistance of the ceramic products after calcination.
[0084] The test results are shown in Table 2.
[0085] Table 2
[0086]
[0087]
[0088] Obviously, for ordinary technicians in the field, other modifications can be made based on the above embodiments, and the obvious modifications brought about by these modifications are still within the protection scope of the present invention.
Claims
1. A ceramic refractory silicone rubber, characterized in that: The following raw materials are included in parts by weight: 50-70 parts of methyl vinyl silicone rubber with a vinyl content of 0.04-0.06%, 30-50 parts of methyl vinyl silicone rubber with a vinyl content of 0.2-0.24%, 20-35 parts of modified silicone rubber, 35-45 parts of fumed silica, 30-40 parts of muscovite, 5-15 parts of glass powder, 3-8 parts of zinc borate, 0.02-0.08 parts of the first catalyst, 1-4 parts of hydrogenated silicone oil, and 1-4 parts of vulcanizing agent.
2. The ceramic refractory silicone rubber according to claim 1, characterized in that: The preparation method of the modified silicone rubber comprises the following steps: 1) mixing hydrogenated silicone rubber, a second catalyst, trichlorovinyl silane and a first organic solvent and reacting them, adding sodium amide after the reaction, continuing the reaction, washing after the reaction, and drying to obtain amino-modified hydrogenated silicone rubber; 2) The amino-modified hydrogenated silicone rubber prepared in step 1), the second organic solvent and water are mixed, ultrasonically dispersed, and then aluminum salt and magnesium salt are added to the ultrasonic dispersion, stirred, and then the pH of the mixed solution is adjusted to 10-13, and the stirring is continued, allowed to stand, filtered, the filter cake is washed with water, and dried to obtain the modified silicone rubber.
3. The ceramic refractory silicone rubber according to claim 2, characterized in that: The mass ratio of the hydrogenated silicone rubber, the second catalyst, trichlorovinyl silane, the first organic solvent and sodium amide is 1: (0.05-0.2): (0.3-0.8): (10-20): (0.32-0.4).
4. The ceramic refractory silicone rubber according to claim 2, characterized in that: The viscosity of the hydrogen-containing silicone rubber is 2000-3000 mPa·s; The second catalyst is catalyst Pt, the first organic solvent is selected from toluene and anhydrous ethanol, and the mass ratio of toluene to anhydrous ethanol is 10:(1-3); The amount of aluminum salt added is 40-65% of the mass of hydrogen-containing silicone rubber, and the amount of magnesium salt added is 15-30% of the mass of hydrogen-containing silicone rubber; The second organic solvent is ethanol, and the mass ratio of the second organic solvent to water is (0.2-0.6):1; In step 2), the amount of the second organic solvent added is 4-7 times the mass of the hydrogen-containing silicone rubber.
5. The ceramic refractory silicone rubber according to claim 2, characterized in that: In step 1), the reaction temperature is 60-75°C, the reaction time is 5-15h, and the continued reaction time is 1-5h; The washing step in step 1) is performed using ethanol and water; In step 2), the stirring temperature is 55-70°C, the stirring time is 0.5-3h, the stirring temperature is continued to be 55-70°C, the stirring time is continued to be 1-3h, the standing temperature is 55-70°C, and the standing time is 3-8h; The ultrasonic dispersion time is 0.5-1.5h, and the ultrasonic power is 200-500W; The pH value of the mixed solution is adjusted to 10-13 using a sodium hydroxide solution with a mass fraction of 8-15%; The aluminum salt is selected from aluminum chloride, and the magnesium salt is selected from magnesium chloride.
6. The ceramic refractory silicone rubber according to claim 1, characterized in that: The first catalyst is composed of diethyl phthalate platinum complex and Raney nickel, and the mass ratio of diethyl phthalate platinum complex to Raney nickel is (1.5-2.5):1; The hydrogen content of the hydrogen-containing silicone oil is 0.1-0.25%, and the viscosity is 100-200 mPa·s; The vulcanizing agent is selected from bis(2,4-dichlorobenzoyl) peroxide.
7. The method for preparing the ceramic refractory silicone rubber according to any one of claims 1 to 6, characterized in that: The steps include: Methyl vinyl silicone rubber with a vinyl content of 0.04-0.06%, methyl vinyl silicone rubber with a vinyl content of 0.2-0.24%, modified silicone rubber and fumed silica are mixed, and muscovite, glass powder, zinc borate, a first catalyst, and hydrogen-containing silicone oil are added after the mixing is completed and the mixing is continued. After the mixing is completed, vacuum is drawn, and then a desulfurizer is added and mixed again, and vulcanization is performed to obtain the ceramicized refractory silicone rubber.
8. The preparation method according to claim 7, characterized in that: The mixing temperature is 80-100°C, the mixing time is 30-60min, the mixing temperature is continued to be 90-110°C, and the mixing time is continued to be 1-3h; The vacuum operation temperature is 120-150℃, and the vacuum time is 20-40min; The mixing time is 20-40 minutes again; The vulcanization temperature is 160-180°C and the vulcanization time is 1-3h.
9. A ceramic fire-resistant silicone rubber foam belt, characterized in that: A ceramic fire-resistant silicone rubber comprising any one of claims 1 to 6; Preferably, the ceramicized refractory silicone rubber foam belt also includes glass cloth.
10. The method for preparing the ceramicized refractory silicone rubber foam tape according to claim 9, characterized in that: The method comprises the following steps: obtaining the ceramicized refractory silicone rubber and glass cloth as described in any one of claims 1 to 6 through a calendering process.
Citation Information
Patent Citations
Flaming retarding highly conductive silicon rubber composite material and preparation method thereof
CN102134399A
Ceramic silicon rubber and preparation method thereof
CN106046797A
Flame-retardant ceramic silicone rubber and preparation method and application thereof
CN109762341A
Silicone rubber composition with fire resistant
KR101896898B1