Preparation method of heat-resistant composite iron oxide green pigment with high solar reflectivity
Through the method of zinc iron phosphate coating iron oxide yellow and direct light-fast turquoise blue GL intercalation zinc aluminum hydrotalcite coating titanium dioxide, combined with bismuth vanadate and titanium dioxide, a composite iron green pigment is formed, which solves the problem of heat resistance of iron oxide green pigment and low reflectivity problem, achieving efficient heat resistance and high solar reflectivity, suitable for high-temperature processing and energy-saving applications.
Patent Information
- Application Number
- CN202410950795.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
AI Technical Summary
Existing iron oxide green pigments have low heat resistance and near-infrared reflectivity and cannot meet the needs of high-temperature processing and energy saving. Moreover, traditional chrome green and phthalocyanine green pigments have problems of toxicity and high cost.
Zinc iron phosphate is used to coat iron oxide yellow, and titanium dioxide is coated with zinc-aluminum hydrotalcite through direct light-fast emerald blue GL intercalation, combined with bismuth vanadate and titanium dioxide to form a composite iron green pigment to improve its heat resistance and solar reflectivity. .
The heat resistance of the composite iron green pigment is increased to above 260°C and the solar reflectivity exceeds 60%, which meets the needs of high-temperature processing and energy-saving applications. The process is simple, low-cost, safe and environmentally friendly.
Smart Images

Figure CN118725612A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pigment production, and in particular to a method for preparing a heat-resistant composite iron green pigment with high solar reflectivity. Background Art
[0002] Plastics are often molded at 140-260°C, and coil coatings are often processed at temperatures above 240°C. The heat resistance of the coloring pigments used must be higher than this temperature to avoid decomposition like organic pigments. Plastic processing, coil coatings, artificial turf and other coloring applications have put forward special requirements for heat-resistant green pigments, so it is imperative to improve the heat resistance of pigments. However, among green pigments, commonly used chrome green pigments are highly toxic and phthalocyanine green pigments are expensive, so it is of great significance to develop low-priced inorganic-organic composite iron green pigments with good heat resistance.
[0003] In terms of roof and wall paint coloring, the use of near-infrared reflective pigments can reflect near-infrared rays in sunlight, thereby effectively reducing heat conduction and achieving energy saving in house air conditioning. Therefore, the research and development of near-infrared reflective pigments has attracted attention. Near-infrared reflective pigments are pigments that present a certain color in the visible light region and have the ability to reflect infrared light in the near-infrared region (700nm~2500nm). They can reduce the surface temperature of objects exposed to sunlight, thereby improving the environment and saving energy.
[0004] Among the existing commercial green pigments, iron oxide green pigment is favored by users due to its safety, environmental protection and moderate price. Iron oxide green pigment is synthesized by using iron oxide yellow and phthalocyanine blue as a composite, which has poor heat resistance and low near-infrared reflectivity. Therefore, improving its heat resistance and near-infrared reflectivity is the key to energy saving, carbon reduction and high-temperature processing application promotion.
[0005] Yellow iron oxide is iron oxide hydroxide, and its chemical formula is usually α-FeOOH. It is widely used in the coating industry, plastic products, construction industry, etc. However, yellow iron oxide has poor thermal stability and begins to lose structural water at around 177°C, so it is greatly restricted in the coloring of plastics and high-temperature coatings.
[0006] The color change trends of the coated iron oxide yellow pigments reported in existing literature and technology after heating are that the L value decreases, the a value increases, and the b value decreases, that is, the red phase of the pigment increases, the yellow phase decreases, and the color darkens after heating. The inventors have discovered that an iron phosphate substance has a reverse change in yellowing (i.e., an increase in b value) when heated (a method for optimizing the heat resistance of coated iron oxide yellow pigments, ZL202210082728.8), which can effectively improve the heat resistance of iron yellow pigments. However, pigments with reverse changes in color Lab values after heating have not been discovered. In addition, the solar reflectivity of existing iron oxide green pigments is very low, often below 35%, and cannot effectively reduce heat conduction. Summary of the invention
[0007] In view of this, the object of the present invention is to provide a method for preparing a heat-resistant composite iron oxide green pigment with high solar reflectivity, so as to prepare a composite iron oxide green pigment with good heat resistance and high solar reflectivity.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] A method for preparing a heat-resistant composite iron green pigment with high solar reflectivity, wherein zinc iron phosphate-coated iron oxide yellow, bismuth vanadate, and titanium dioxide are mixed in a mass ratio of 1:0.1-0.5:0.1-0.5, and then directly coated with a light-resistant turquoise blue GL intercalated zinc aluminum hydrotalcite surface to obtain a composite iron green pigment. The composite iron green pigment has a solar reflectivity of more than 60% and a heat resistance of up to 260°C.
[0010] Preferably, zinc phosphate-coated yellow iron oxide, bismuth vanadate, and titanium dioxide are mixed in a mass ratio of 1:0.1-0.5:0.1-0.5, and then 4 g of the mixture of zinc phosphate-coated yellow iron oxide, bismuth vanadate, and titanium dioxide is weighed, 400 mL of water is added, and stirred in a water bath at 80 ° C for 30 min; 0.73 g Zn(NO 3 ) 2 6H 2 O and 0.31g Al(NO 3 ) 3 9H 2 100mL aqueous solution prepared by O and 100mL aqueous solution prepared by 0.26g NaOH were added dropwise for 20min, and the pH value of the solution was kept between 9 and 10. After the addition was completed, stirring was continued for 30min, crystallized in an 80℃ oven for 24h, and then stirred in an 80℃ water bath for 30min, 0.32g direct light-fast turquoise blue GL was added and stirred for 1h, and the composite iron green pigment was obtained by suction filtration, washing, drying and crushing.
[0011] Preferably, weigh 20g of yellow iron oxide pigment 810#, and evenly disperse the yellow iron oxide in 200mL of water under stirring to form a mixed solution with a yellow iron oxide content of 10%; weigh 3.05g of ZnCl 2 , 0.32gFeSO 4 7H 2 O, 2.53 g (NaPO 3 ) 6, 1.64g NaOH, dissolved in 100L water respectively to prepare solution A, solution B and solution C; then add solution A, solution B and solution C into the yellow iron oxide mixture while stirring, the reaction temperature is controlled at 80℃, and stirring is continued for 3h after the solution is added; after suction filtration and washing, the filter cake is dried and crushed at 90℃ to obtain zinc iron phosphate coated yellow iron oxide.
[0012] The present invention has the following beneficial effects due to the adoption of the above technical solution:
[0013] 1. This patent achieves improved heat resistance of iron oxide yellow pigment by coating iron zinc phosphate, which can reach above 260°C to meet the application requirements of heat-resistant iron oxide green pigment.
[0014] 2. The direct sun-resistant turquoise blue GL intercalated zinc-aluminum hydrotalcite coated titanium dioxide discovered in this patent has just the color-complementing function, which can effectively improve the heat resistance of iron yellow pigment. By further coating the surface of iron yellow with blue substances, the design of green iron-based pigments can be realized, which is beneficial to the preparation of iron green pigments with excellent heat resistance.
[0015] 3. This patent proposes that on the basis of coated yellow iron oxide, bismuth vanadate and titanium dioxide with high reflectivity are added to effectively control the yellow tone and near-infrared reflectivity, thereby achieving high solar reflectivity and color adjustability after direct heat-resistant turquoise intercalated zinc-aluminum hydrotalcite coating.
[0016] 4. The preparation method of the composite iron green pigment invented by this patent has the advantages of simple synthesis method, low cost, safety and environmental protection. The green pigment product produced has a solar reflectivity of more than 60% and a heat resistance of 260°C. It can meet the coloring and energy-saving application needs of plastic processing, coil coatings, artificial turf, etc., can save energy and reduce consumption, and has a high industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the chromaticity diagram of composite iron green pigment 2# before and after baking;
[0018] Figure 2 It is the UV-Vis-NIR spectra of direct light-fast turquoise blue GL intercalated zinc-aluminum hydrotalcite coated with titanium dioxide, composite iron green pigment 2# and zinc iron phosphate coated iron oxide yellow. DETAILED DESCRIPTION
[0019] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
[0020] Example 1
[0021] Preparation method of zinc iron phosphate coated iron oxide yellow: weigh 20g of iron oxide yellow pigment 810#, and evenly disperse the iron oxide yellow in 200mL of water under stirring to form a mixed solution with an iron oxide yellow content of 10%; weigh 3.05g ZnCl 2 , 0.32gFeSO 4 7H 2 O, 2.53 g (NaPO 3 ) 6 , 1.64g NaOH, dissolved in 100L water respectively to prepare solution A, solution B and solution C; then add solution A, solution B and solution C into the yellow iron oxide mixture while stirring, the reaction temperature is controlled at 80℃, and stirring is continued for 3h after the solution is added; after suction filtration and washing, the filter cake is dried and crushed at 90℃ to obtain zinc iron phosphate coated yellow iron oxide.
[0022] Example 2
[0023] Preparation method of composite iron green pigment: zinc phosphate coated iron oxide yellow, bismuth vanadate, and titanium dioxide are mixed in a mass ratio of 1:0.1:0.1, then 4g of the mixture of zinc phosphate coated iron oxide yellow, bismuth vanadate, and titanium dioxide is weighed, 400mL of water is added, and stirred in a water bath at 80°C for 30min; 0.73gZn(NO 3 ) 2 6H 2 O and 0.31g Al(NO 3 ) 3 9H 2 100mL aqueous solution prepared by O and 100mL aqueous solution prepared by 0.26g NaOH were added dropwise for 20min at the same time, and the pH value of the solution was kept between 9 and 10. After the addition was completed, stirring was continued for 30min, crystallized in an 80℃ oven for 24h, and then stirred in an 80℃ water bath for 30min, 0.32g direct light-fast turquoise blue GL was added and stirred for 1h, and then filtered, washed, dried and crushed to obtain composite iron green pigment 1#.
[0024] Example 3
[0025] Preparation method of composite iron green pigment: zinc phosphate coated iron oxide yellow, bismuth vanadate, and titanium dioxide are mixed in a mass ratio of 1:0.2:0.3, then 4g of the mixture of zinc phosphate coated iron oxide yellow, bismuth vanadate, and titanium dioxide is weighed, 400mL of water is added, and stirred in a water bath at 80°C for 30min; 0.73gZn(NO 3 ) 2 6H 2 O and 0.31g Al(NO 3 ) 3 9H 2100mL aqueous solution prepared by O and 100mL aqueous solution prepared by 0.26g NaOH were added dropwise for 20min at the same time, and the pH value of the solution was kept between 9 and 10. After the addition was completed, stirring was continued for 30min, crystallized in an 80℃ oven for 24h, and then stirred in an 80℃ water bath for 30min, 0.32g direct light-fast turquoise blue GL was added and stirred for 1h, and then filtered, washed, dried and crushed to obtain composite iron green pigment 2#.
[0026] Example 4
[0027] Preparation method of composite iron green pigment: zinc phosphate coated iron oxide yellow, bismuth vanadate, and titanium dioxide are mixed in a mass ratio of 1:0.5:0.5, then 4g of the mixture of zinc phosphate coated iron oxide yellow, bismuth vanadate, and titanium dioxide is weighed, 400mL of water is added, and stirred in a water bath at 80°C for 30min; 0.73gZn(NO 3 ) 2 6H 2 O and 0.31g Al(NO 3 ) 3 9H 2 100mL aqueous solution prepared by O and 100mL aqueous solution prepared by 0.26g NaOH were added dropwise for 20min at the same time, and the pH value of the solution was kept between 9 and 10. After the addition was completed, stirring was continued for 30min, crystallized in an 80℃ oven for 24h, and then stirred in an 80℃ water bath for 30min, 0.32g direct light-fast turquoise blue GL was added and stirred for 1h, and then filtered, washed, dried and crushed to obtain composite iron green pigment 3#.
[0028] Example 5
[0029] Comparative experiment:
[0030] Direct light-fast turquoise GL intercalated zinc-aluminum hydrotalcite coated titanium dioxide: weigh 4g titanium dioxide, add 400mL water and stir in a water bath at 80℃ for 30min; then add 0.73gZn(NO 3 ) 2 6H 2 O and 0.31gAl(NO 3 ) 3 9H 2 100 mL aqueous solution prepared with 0.26 g of NaOH and 100 mL aqueous solution prepared with 0.26 g of NaOH were added dropwise for 20 min in a water bath at 80 ° C with stirring, and the pH value of the solution was kept between 9 and 10. After the addition was completed, stirring was continued for 30 min, crystallized in an oven at 80 ° C for 24 h, and then stirred in a water bath at 80 ° C for 30 min, 0.32 g of direct light-fast turquoise blue GL was added and stirred for 1 h, and then filtered, washed, dried, and crushed to obtain direct light-fast turquoise blue GL intercalated zinc-aluminum hydrotalcite coated titanium dioxide.
[0031] Example 6
[0032] The composite iron green pigments 1#, 2#, and 3# were tested for heat resistance at 260°C. The test method is as follows: weigh 2g of the product, put it into a small crucible, heat it in a 260°C oven for 0.5h, take it out and cool it. The color difference values ΔE of the composite iron green pigments 1#, 2#, and 3# tested on the spectrophotometer are 1.75, 1.52, and 1.68 respectively, indicating that the heat resistance of the three samples can reach 260°C. The chromaticity diagram of the composite iron green pigment 2# before and after baking is attached. Figure 1 , wherein a is the composite iron green pigment 2# before baking; b is the composite iron green pigment 2# after baking.
[0033] Thermal color correction verification experiment: The heat resistance of zinc phosphate coated yellow iron oxide was tested at 260°C. The Lab values before baking were 63.35, 14.63, and 37.08, respectively. The Lab values after baking were 63.05, 15.14, and 36.72, respectively. The color difference value ΔE was 0.69, indicating that zinc phosphate coated yellow iron oxide has high heat resistance; the direct light-fast turquoise GL intercalated zinc-aluminum hydrotalcite coated titanium dioxide in Example 5 was tested for heat resistance at 260°C. The Lab values before baking were 70.20, -18.07, -20.92, and the Lab values after baking are 71.08, -19.42, -16.15 respectively, and the color difference value ΔE is 5.04; compared with the two, the ΔL value of the coated iron oxide yellow decreases, the Δa value increases, and the Δb value decreases after heating; while the color change of direct light-fast turquoise blue GL intercalated zinc-aluminum hydrotalcite coated titanium dioxide is just the opposite, so the two play a complementary role in the change of color Lab value after heating. After the two are coated, the color difference value can be reduced, realizing the color complementation function under heat.
[0034] Example 7
[0035] The spectral data of direct fast turquoise blue GL intercalated zinc aluminum hydrotalcite coated titanium dioxide, composite iron green pigment 2# and zinc iron phosphate coated iron oxide yellow were tested by PerkinElmer LAMBDA 1050+ UV-Vis-NIR spectrophotometer. The UV-Vis-NIR spectra are shown in the attached figure. Figure 2 , and calculate its solar reflectivity.
[0036] The spectral data in the figure can be used to calculate that the solar reflectances of zinc iron phosphate coated iron oxide yellow and direct light-fast turquoise GL intercalated zinc aluminum hydrotalcite coated titanium dioxide are 56.4% and 64.8% respectively, and the solar reflectance of composite iron green pigment 2# is 60.5%. Using the same method, the solar reflectances of composite iron green pigments 1# and 3# are measured to be 60.1% and 60.3% respectively.
[0037] The composite iron green pigment invented in this patent has high solar reflectivity and excellent heat resistance. It can be used as a colorant for plastic processing and powder coatings at 260°C, and has the advantages of energy saving and carbon reduction.
Claims
1. A method for preparing a heat-resistant composite iron green pigment with high solar reflectivity, characterized in that: Zinc iron phosphate coated yellow iron oxide, bismuth vanadate and titanium dioxide are mixed in a mass ratio of 1:0.1-0.5:0.1-0.5, and then directly coated on the surface of light-fast turquoise blue GL intercalated zinc aluminum hydrotalcite to obtain a composite iron green pigment. The composite iron green pigment has a solar reflectivity of more than 60% and a heat resistance of up to 260°C.
2. A method for preparing a heat-resistant composite iron green pigment with high solar reflectivity as claimed in claim 1, characterized in that: Zinc phosphate-coated yellow iron oxide, bismuth vanadate and titanium dioxide are mixed in a mass ratio of 1:0.1-0.5:0.1-0.5, then 4g of the mixture of zinc phosphate-coated yellow iron oxide, bismuth vanadate and titanium dioxide is weighed, 400mL of water is added and stirred in a water bath at 80°C for 30min; 100mL of an aqueous solution prepared by 0.73g of Zn(NO3)2·6H2O and 0.31g of Al(NO3)3·9H2O and 100mL of an aqueous solution prepared by 0.26g of NaOH are simultaneously added dropwise for 20min, and the pH value of the solution is maintained between 9 and 10; after the addition is completed, stirring is continued for 30min, crystallized in an oven at 80°C for 24h, then stirred in a water bath at 80°C for 30min, 0.32g of direct light-fast turquoise blue GL is added and stirred for 1h, and the composite iron green pigment is obtained by suction filtration, washing, drying and crushing.
3. A method for preparing a heat-resistant composite iron green pigment with high solar reflectivity as claimed in claim 1, characterized in that: The preparation method of the zinc iron phosphate coated yellow iron oxide is as follows: weigh 20g of yellow iron oxide pigment 810#, and evenly disperse the yellow iron oxide in 200mL of water under stirring to form a mixed solution with an iron oxide yellow content of 10%; weigh 3.05g of ZnCl2, 0.32g of FeSO4·7H2O, 2.53g of (NaPO3)6, and 1.64g of NaOH, and dissolve them in 100L of water respectively to prepare solution A, solution B, and solution C; then add solution A, solution B, and solution C to the yellow iron oxide mixed solution under stirring at the same time, control the reaction temperature at 80°C, and continue stirring for 3h after the solution is added; after suction filtration and washing, dry and crush the filter cake at 90°C to obtain the zinc iron phosphate coated yellow iron oxide.